A refining method and lignin technology, which is applied to the chemical characteristics of fibers, textiles and papermaking, etc., can solve the problems of low lignin extraction rate, complex and cumbersome lignin treatment, and low purity, so as to improve economic and social benefits, and operate Convenience, effect of improving purity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A method for extracting and refining lignin used for carbon fiber preparation, comprising the steps of:
[0022] a. Put the wood in a grinder and crush it into 50-mesh powder, dissolve the powder in polyol, add hydrochloric acid to adjust the pH to 3, stir and react at 180°C for 35 minutes to obtain the stock solution, and the polyol is distilled and recycled;
[0023] b. Add 60 times the volume of distilled water to the stock solution obtained in step a, and heat up from room temperature to 150°C within 15 minutes for cellulose regeneration. The regeneration time is 2 hours, and the stock solution is cooled to 20°C before fiber regeneration;
[0024] c. Separating the liquid treated in step b to obtain a filtrate system, so that polyhydric alcohol, hydrochloric acid and distilled water are separated into the filtrate system;
[0025] d. The filtrate system obtained in step c is dissolved in cyclohexane and left to stand until all the lignin is precipitated, and the cyc...
Embodiment 2
[0029] A method for extracting and refining lignin used for carbon fiber preparation, comprising the steps of:
[0030] a. Put the wood in a pulverizer and pulverize it into 100-mesh powder, dissolve the powder in polyol, add sulfuric acid to adjust the pH to 4, stir and react at 200°C for 45 minutes to obtain the stock solution, and the polyol is distilled and recycled for reuse;
[0031] b. Add 80 times the volume of distilled water to the stock solution obtained in step a, and heat up from room temperature to 150°C within 20 minutes for cellulose regeneration. The regeneration time is 4 hours, and the stock solution is cooled to 40°C before fiber regeneration;
[0032] c. separating the liquid treated in step b to obtain a filtrate system, so that polyhydric alcohol, sulfuric acid and distilled water are separated into the filtrate system;
[0033] d, dissolving the filtrate system obtained in step c in dichloromethane and standing until the lignin is completely precipitate...
Embodiment 3
[0037] A method for extracting and refining lignin used for carbon fiber preparation, comprising the steps of:
[0038] a. Put the wood in a pulverizer and pulverize it into 100-mesh powder, dissolve the powder in polyol, add phosphoric acid to adjust the pH to 4.5, stir and react at 200°C for 60 minutes to obtain the stock solution, and the polyol is distilled and recycled for reuse;
[0039] b. Add 100 times the volume of distilled water to the stock solution obtained in step a, and heat up from room temperature to 150°C within 25 minutes for cellulose regeneration. The regeneration time is 6 hours, and the stock solution is cooled to 55°C before fiber regeneration;
[0040] c. Separating the liquid treated in step b to obtain a filtrate system, so that polyhydric alcohol, phosphoric acid and distilled water are separated into the filtrate system;
[0041] d, dissolving the filtrate system obtained in step c in a mixed solution of cyclohexane and dichloromethane and standing...