A slope protection and road technology, applied in excavation, construction, infrastructure engineering, etc., can solve the problems of time-consuming impact, complex construction, and affecting the aesthetics of high slopes, and achieve simple methods, crack resistance and freeze-thaw resistance powerful effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] A method for protecting road high slopes, comprising the following steps:
[0036] (1) High slope trimming;
[0037] (2) Anchor rod construction: Drill to the design depth, insert the anchor rod and perform pressure grouting. The slurry is cement mortar with a weight ratio of cement, sand and water of 1:3:0.6, and the pressure is 0.4MPa;
[0038] (3) Foundation excavation and steel bar binding;
[0039] (4) Build templates;
[0040] (5) Concrete pouring: Concrete is counted in parts by weight, including: 180 parts of cement, 300 parts of gravel, 200 parts of river sand, 5 parts of cotton fiber, 50 parts of fly ash, 15 parts of activated carbon and 100 parts of water;
[0041] Wherein, the preparation method of concrete comprises the following steps:
[0042] S1. Stir cement, gravel, river sand and water, the stirring speed is 30r / min, and the stirring time is 20min to obtain a mixture A, and mix fly ash and activated carbon to obtain a mixture B;
[0043] S2. Cut th...
Embodiment 2
[0049] A method for protecting road high slopes, comprising the following steps:
[0050] (1) High slope trimming;
[0051] (2) Anchor construction: Drill to the design depth, insert the anchor and perform pressure grouting. The slurry is cement mortar with a weight ratio of cement, sand and water of 1:3:0.6, and the pressure is 0.5MPa;
[0052] (3) Foundation excavation and steel bar binding;
[0053] (4) Build templates;
[0054] (5) Concrete pouring: Concrete is calculated in parts by weight, including: 250 parts of cement, 400 parts of gravel, 320 parts of river sand, 7 parts of cotton fiber, 80 parts of fly ash, 30 parts of activated carbon and 150 parts of water;
[0055] Wherein, the preparation method of concrete comprises the following steps:
[0056]S1. Stir cement, gravel, river sand and water, the stirring speed is 35r / min, and the stirring time is 30min to obtain a mixture A, and mix fly ash and activated carbon to obtain a mixture B;
[0057] S2. Cut the cott...
Embodiment 3
[0063] A method for protecting road high slopes, comprising the following steps:
[0064] (1) High slope trimming;
[0065] (2) Anchor rod construction: Drill to the design depth, insert the anchor rod and perform pressure grouting. The slurry is cement mortar with a weight ratio of cement, sand and water of 1:3:0.6, and the pressure is 0.6MPa;
[0066] (3) Foundation excavation and steel bar binding;
[0067] (4) Build templates;
[0068] (5) Concrete pouring: Concrete is counted in parts by weight, including: 220 parts of cement, 360 parts of gravel, 280 parts of river sand, 6 parts of cotton fiber, 65 parts of fly ash, 21 parts of activated carbon and 130 parts of water;
[0069] Wherein, the preparation method of concrete comprises the following steps:
[0070] S1. Stir cement, gravel, river sand and water, the stirring speed is 32r / min, and the stirring time is 25min to obtain mixture A, and mix fly ash and activated carbon to obtain mixture B;
[0071] S2. Cut the co...