[0003] Existing sealant compositions are prone to sagging or tailing during use
Smearing phenomenon, that is, using a glue gun to apply the sealant on the weld seam. When the required length of glue extrusion is completed, the gun is lifted. Due to the viscosity of the glue and the inertia of extrusion, there is still a part of the glue remaining on the car body. The phenomenon is called tailing phenomenon, which leads to unsightly bonding, and after a long time, the sealant is prone to aging and yellowing

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Sealant composition

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0024] see figure 1 , the invention provides a sealant composition, which is formed by the following raw material ratio in parts by weight: 100 parts of base material, 20 parts of modified filler, 0.3 part of expanded microspheres, 6 parts of thixotropic agent, light stabilizer 0.5 parts, 0.5 parts of coupling agent, 3 parts of curing agent, 10 parts of plasticizer, 0.5 parts of catalyst and 2 parts of adhesion promoter.

[0025] Specifically, the base material is mainly prepared from the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 30 parts of white carbon black, 5 parts of treatment agent, 3 parts of anti-aging agent and 5 parts of water.

[0026] Specifically, vinyl silicone oil is mainly prepared from the following raw materials in parts by weight: 800 parts of octamethylcyclotetrasiloxane, 12 parts of methyltrimethoxysilane, 16 parts of tetramethyldivinylsilicyloxane and Catalyst A 0.1 part.

[0027] Specifically, the modified filler is o...

Embodiment 2

[0035] see figure 1 , the invention provides a sealant composition, which is formed by the following raw material ratio in parts by weight: 100 parts of base material, 30 parts of modified filler, 0.5 part of expanded microspheres, 15 parts of thixotropic agent, light stabilizer 2 parts, 3 parts of coupling agent, 4 parts of curing agent, 15 parts of plasticizer, 2 parts of catalyst and 5 parts of adhesion promoter.

[0036] Specifically, the base material is mainly prepared from the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 60 parts of white carbon black, 14 parts of treatment agent, 12 parts of anti-aging agent and 7 parts of water.

[0037] Specifically, vinyl silicone oil is mainly prepared from the following raw materials in parts by weight: 800 parts of octamethylcyclotetrasiloxane, 15 parts of methyltrimethoxysilane, 20 parts of tetramethyldivinylsilicyloxane and 0.3 parts of catalyst A.

[0038] Specifically, the modified filler is ...

Embodiment 3

[0046] see figure 1 , the invention provides a sealant composition, which is formed by the following raw material ratio in parts by weight: 100 parts of base material, 40 parts of modified filler, 0.9 part of expanded microspheres, 20 parts of thixotropic agent, light stabilizer 3 parts, 5 parts of coupling agent, 5 parts of curing agent, 20 parts of plasticizer, 3 parts of catalyst and 8 parts of adhesion promoter.

[0047] Specifically, the base material is mainly prepared from the following raw materials in parts by weight: 100 parts of vinyl silicone oil, 100 parts of white carbon black, 20 parts of treatment agent, 18 parts of anti-aging agent and 10 parts of water.

[0048] Specifically, vinyl silicone oil is mainly prepared from the following raw materials in parts by weight: 800 parts of octamethylcyclotetrasiloxane, 19 parts of methyltrimethoxysilane, 27 parts of tetramethyldivinylsilicyloxane and 0.4 parts of catalyst A.

[0049] Specifically, the modified filler i...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
particle diameteraaaaaaaaaa
particle diameteraaaaaaaaaa
Login to view more

Abstract

The invention belongs to the technical field of sealants, and particularly discloses a sealant composition which is prepared from the following raw materials in parts by weight: 100 parts of a base material, 20-40 parts of modified filler, 0.3-0.9 part of expanded microspheres, 6-20 parts of a thixotropic agent, 0.5-3 parts of a light stabilizer, 0.5-5 parts of a coupling agent, 3-5 parts of a curing agent, 10-20 parts of a plasticizer, 0.5-3 parts of a catalyst and 2-8 parts of an adhesion promoter, the expanded microspheres with large volume and small mass are used as the light filler, an excellent weight reduction effect can be achieved by adding a small amount of the expanded microspheres, the density of the sealant is remarkably reduced, the sealant is convenient to transport, a small amount of the expanded microspheres can replace most of raw materials, and the production and transportation cost is greatly reduced; the ultraviolet absorbent, the light stabilizer and the antioxidant are effectively compounded through structure optimization to obtain the light stabilizer, the problem that the sealant is resistant to yellowing after being used for a long time is solved, and meanwhile, the tea polyphenol type antioxidant introduced into the light stabilizer also has antibacterial and mildew-proof effects.

Description

technical field [0001] The invention belongs to the technical field of sealants, and in particular relates to a sealant composition. Background technique [0002] Sealant is a sealing material that bonds the surfaces of the same or different solid materials together, or is used to fill the gaps in the material, and acts as a sealant. It is a kind of adhesive that is leak-proof, waterproof, Anti-vibration and heat insulation, sound insulation and other functions. Sealants have been widely used in aerospace, automobile transportation, machinery manufacturing, material processing, electronic appliances, national defense and military industry, building materials, petrochemical industry, printing and binding, light industry and textile, medical and health care, and daily life. [0003] The existing sealant composition is prone to sagging or tailing phenomenon during use. Smearing phenomenon, that is, using a glue gun to apply the sealant on the weld seam. When the required leng...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C09J183/07C09J11/04C09J11/06C09J11/08
Inventor 王勇
Owner 常州科菲自动化科技有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products