Finishing method of single-absorption and single-prevention fabric
A waterproof finishing and fabric technology, applied in fiber processing, textiles and papermaking, etc., can solve the problems of only moisture absorption and perspiration function, only waterproof function, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0014] The component ratio of the waterproof finishing liquid is by weight:
[0015] Rudolph fluorocarbon resin FC-9005 140 parts;
[0016] Rudolph cross-linking agent FX-8005 11 parts;
[0017] Rudolf thickener TH-5000 800 parts;
[0018] (1), water absorption finishing: dyed 170 g / m 2 The pure polyester cotton wool fabric is soaked in the hydrophilic finishing solution for 5 minutes, the pH value of the impregnation is 4.5, the soaking temperature is room temperature, and the bath ratio is 1:10; the amount of the hydrophilic additive in the hydrophilic finishing solution is 10 g / L, and the rest Water; the soaked fabric is rolled dry at a pressure of 7kg / cm 2 , with a liquid retention rate of 70%; dry the dried fabric at 130°C;
[0019] (2) Waterproof finishing: apply waterproof finishing solution on the rotary screen printing machine on the front of the fabric finished by the water absorption in step (1), the temperature is 150° C., and the time is 2 minutes.
Embodiment 2
[0021] The component ratio of the waterproof finishing liquid is by weight:
[0022] Rudolph fluorocarbon resin FC-9005 150 parts;
[0023] Rudolph cross-linking agent FX-8005 10 parts;
[0024] Rudolf thickener TH-5000 820 parts;
[0025] (1) Water absorption finishing: the dyed 180 g / m 2 The pure cotton jersey is soaked in the hydrophilic finishing solution for 10 minutes, the dipping pH value is 4.5, the soaking temperature is room temperature, and the bath ratio is 1:30; the amount of hydrophilic additive in the hydrophilic finishing solution is 15 grams per liter, and the rest is Water; the soaked fabric is rolled dry at a pressure of 5kg / cm 2 , with a liquid retention rate of 75%; dry the dried fabric at 140°C;
[0026] (2) Waterproof finishing: apply waterproof finishing liquid on the rotary screen printing machine on the front of the fabric that has been water-absorbed in step (1), at a temperature of 160° C. for 1.5 minutes.
Embodiment 3
[0028] The component ratio of the waterproof finishing liquid is by weight:
[0029] Rudolph fluorocarbon resin FC-9005 160 parts;
[0030] Rudolph cross-linking agent FX-8005 11 parts;
[0031] Rudolf thickener TH-5000 840 parts;
[0032] (1), water absorption finishing: the dyed 190 g / m 2 The all-polyester mesh cloth is soaked in the hydrophilic finishing solution for 15 minutes, the dipping pH value is 5, the soaking temperature is room temperature, and the bath ratio is 1:50; the amount of hydrophilic additive in the hydrophilic finishing solution is 20 g / L, and the rest is Water; the soaked fabric is rolled dry at a pressure of 3kg / cm 2 , with a liquid retention rate of 80%; dry the dried fabric at 160°C;
[0033] (2) Waterproof finishing: apply waterproof finishing liquid on the front of the fabric that has been water-absorbed in step (1) on a rotary screen printing machine at a temperature of 170° C. for 1 minute.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com