Wood craft grinding and blackening antique imitation process
A handicraft and wood technology, which is applied in the field of blackening and antique crafting of wooden handicrafts, can solve the problems of poor coloring effect, low processing efficiency of handicraft lines, difficult surface coloring, etc., and achieves beautiful decolorization, easy implementation, and difficult decolorization. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] A kind of wooden handicraft of the present invention grinds black and imitates the antique craft, comprises steps as follows:
[0023] (1) Beat the wood and polish it;
[0024] (2) Use the high-speed rotating grinding head to grind the wood surface. During the grinding process, the heat generated by the high-speed friction between the grinding wheel and the wood will carbonize the wood surface;
[0025] (3) Clean the surface of the carbonized wood, and then evenly coat the surface treatment agent on the surface of the wood, bake it, dry it, and then polish it.
[0026] In the process step (2), the diameter of the cross-section of the grinding wheel head is 5mm-30mm, so as to meet the needs of engraving lines of various sizes on different parts of the surface of the handicraft.
[0027] In the process step (2), the grinding wheel head is spherical or conical or barbell-shaped. The spherical grinding wheel head can be used to rub the concave part of the surface of the ha...
Embodiment 2
[0034] The difference between this embodiment and Example 1 is: the surface treatment agent comprises the following components by weight percentage: white mineral wax 15.8%, beeswax 15.8%, turpentine 62.4%, raw lacquer 3%, rosin 3%, weight respectively White mineral wax 15.8g, beeswax 15.8g, turpentine 62.4g, lacquer 3g, rosin 3g. The preparation method of the surface treatment agent, its steps are as follows: mix white mineral wax and beeswax by weight ratio 1:1, and melt under the heating of 100 degree electric hot air, and after being oily, add turpentine again, described The weight of turpentine added is twice the weight of white mineral wax and beeswax, then raw lacquer and rosin are added, and the surface treatment agent is prepared after stirring.
Embodiment 3
[0036] The difference between this embodiment and Example 1 is: the surface treatment agent comprises the following components by weight percentage: white mineral wax 15.3%, beeswax 15.3%, turpentine 61.2%, lacquer 4.1%, rosin 4.1%, weight respectively White mineral wax 15.3g, beeswax 15.3g, turpentine 61.2g, lacquer 4.1g, rosin 4.1g. The preparation method of the surface treatment agent, its steps are as follows: white mineral wax and beeswax are mixed by weight ratio 1:1, and melt under the heating of 60 degree electric hot air, and after being oily, add turpentine again, described The weight of turpentine added is twice the weight of white mineral wax and beeswax, then raw lacquer and rosin are added, and the surface treatment agent is prepared after stirring.
[0037] It should be pointed out that the grinding wheel of the present invention can be processed into various desired shapes according to needs, such as cone, ball, dish, etc. as mentioned above, so as to better ca...