Brown coal floatation method
A technology for lignite and upgraded coal, which is used in flotation, solid separation, petroleum industry, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] This embodiment discloses a lignite flotation method. Lignite from the Yuanbaoshan Mining Area in Chifeng City, Inner Mongolia is selected as a raw material, and conventional flotation equipment is used. The lignite flotation method described in this embodiment specifically includes the following steps:
[0034] First, the upgraded coal obtained by subjecting lignite to low-temperature pyrolysis (thermal upgrading) at 300°C has an ash content of 17.13%; after the upgraded coal is crushed to a particle size of less than 0.5mm, it is configured into The concentration of the pulp is 60g / L, the mixing speed of the pulp is 2100r / min, and the air volume is 300L / h. The collision between the upgraded coal particles and the air bubbles will make the upgraded coal particles adhere to the surface of the air bubbles in time and separate from the tailing coal or ash. separation;
[0035] Then, pre-stirring for 2min, adding kerosene to the slurry, the amount of kerosene added is 3.5k...
Embodiment 2
[0039] This embodiment discloses a lignite flotation method. Lignite from the Yuanbaoshan mining area in Chifeng City, Inner Mongolia is selected as a raw material, and conventional flotation equipment is used. The lignite flotation method described in this embodiment specifically includes the following steps:
[0040] First, the upgraded coal obtained by subjecting lignite to low-temperature pyrolysis (thermal upgrading) at 400°C has an ash content of 18.87%; after the upgraded coal is crushed to a particle size of less than 0.5mm, it is configured into The concentration of the pulp is 60g / L, and the mixing speed of the configured pulp is: 2100r / min, and the aeration volume is 300L / h;
[0041] Then, pre-stirring for 2min, adding kerosene to the slurry, the amount of kerosene added is 3.5kg / t;
[0042] Finally, stir for 1 min, then add 2-octanol to the pulp, the amount of 2-octanol added is 0.462kg / t, after 10s, scrape at a speed of 30r / min for 3min, and control the water repl...
Embodiment 3
[0045] This embodiment discloses a lignite flotation method. Lignite from the Yuanbaoshan mining area in Chifeng City, Inner Mongolia is selected as a raw material, and conventional flotation equipment is used. The lignite flotation method described in this embodiment specifically includes the following steps:
[0046] First, the upgraded coal obtained by subjecting lignite to low-temperature pyrolysis (thermal upgrading) at 500°C has an ash content of 20.84%; after the upgraded coal is crushed to a particle size of less than 0.5mm, it is configured into The concentration of the pulp is 60g / L, and the mixing speed of the configured pulp is: 2100r / min, and the aeration volume is 300L / h;
[0047] Then, pre-stirring for 2min, adding kerosene to the slurry, the amount of kerosene added is 3.5kg / t;
[0048]Finally, stir for 1 min, then add 2-octanol to the pulp, the amount of 2-octanol added is 0.462kg / t, after 10s, scrape at a speed of 30r / min for 3min, and control the water reple...