Embodiment 1
[0039] Preparation of 1# degradable micro-lubricating oil
[0040] Take early fried dough sticks and filter to remove impurities, weigh 885g (calculated as 1mol based on triglyceride) and put it in the reactor, weigh 92g (2mol) of ethanol, add 1.77g of sodium hydroxide into the reactor, and put it into the reactor at 70°C Sealed and stirred for 90 minutes, added 71g (0.5mol) of phosphorus pentoxide and continued to stir for 60 minutes to fully react, and naturally cooled to obtain 1# degradable trace lubricating oil.
Embodiment 2
[0042] Preparation of 2# degradable micro-lubricating oil
[0043] Put the pig fat outside (20-30°C) for 2 days. When there is already an odor, put it in a pot to heat and fry it, filter out impurities, weigh 885g (calculated as 1mol based on triglyceride) and set In the reactor, weigh 88g (1mol) of n-pentanol, add 4.425g of sodium ethoxide into the reactor, seal and stir at 90°C for 60 minutes, add 142g (1mol) of phosphorus pentoxide and continue to stir for 90 minutes to fully react , cooled naturally to obtain a lubricant composition.
[0044] Add 200g soybean oil, 200g methyl palmitate, 100g dioctyl sebacate, 100g pentaerythritol tetralaurate, 100g polyalpha-olefin (PAO4) in the above-mentioned lubricating oil composition and fully stir for 20 minutes , to produce 2# degradable micro-lubricating oil.
Embodiment 3
[0046] Preparation of 3# degradable micro-lubricating oil
[0047] Add 1000 grams of Arowana blended oil to 2000 grams of water, 100 grams of fish, 200 grams of tofu, 200 grams of Chinese cabbage, 20 grams of pepper, 10 grams of Zanthoxylum bungeanum, put it in a pot and cook for 2 hours, filter to remove impurities, and separate oil and water with BY-1 Remove moisture by machine, weigh 885g (calculated as 1mol based on triglyceride) and put it in the reactor, weigh 90g (1.5mol) propanol, add 3g potassium methylate into the reactor, seal and stir for 75 minutes at 80°C , add 97g (1mol) of phosphoric acid and continue to stir to make it fully react for 80 minutes, and cool naturally to obtain a lubricant composition.
[0048] Add 500 g of trimethylolpropane oleate and 50 g of tributyl borate to the above lubricant composition, and stir well until the solution is completely transparent to obtain 3# degradable trace lubricating oil.