A sea cucumber polypeptide and edible film technology, which is applied to the field of oral sea cucumber biological active substances, can solve the problems of inability to show effects, inconvenient taking forms, etc., and achieve the effects of good removal effect, convenient carrying and eating.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0043]
[0044] A kind of anti-drowsiness sea cucumber edible film and the process of making method thereof:
[0045] 1. First add 1572g of pure water into a 10L stainless steel batching tank (Wenzhou Haichuan Machinery Co., Ltd.), and then slowly put the sea cucumber polypeptide powder 1080 (≤2000D) extracted by biological enzymatic hydrolysis into the pure water For dissolving, heat to 50° C. to dissolve faster to obtain 2652 g of sea cucumber polypeptide powder dissolving solution.
[0046] 2. Add 1179g of purified water into a 10L stainless steel batching tank (Wenzhou Haichuan Machinery Co., Ltd.), add 300g of American ginseng powder and 102g of mint leaf powder respectively, and stir evenly to obtain 1581g of a mixed solution of American ginseng powder and mint leaf powder.
[0047] 3. Add 4233g of the two solutions into a 10L stainless steel batching tank (Wenzhou Haichuan Machinery Co., Ltd.), mix well, then add 300g of glucose and dissolve.
[0048] 4. Dissolve 30...
Embodiment 2
[0060]
[0061] 1) Mixing and dissolving: ①Mix in one unit; in a 10L stainless steel batching tank (Wenzhou Haichuan Machinery Co., Ltd.), heat 1200g of sea cucumber polypeptide powder with 1572g of pure water at 40°C to dissolve according to the metering ratio, then add 120g of American ginseng powder and mint leaf powder 90g was dissolved in 1572g water respectively and mixed with 2770g sea cucumber polypeptide powder dissolving solution and stirred uniformly, 480g glucose was added thereto, and after glucose was dissolved, 5034g mixed dissolving solution was obtained;
[0062] ② Two unit mixing; use 5L triangular flask to add 12g of peppermint oil and 18g of lemon essential oil into 530g of 5.7% (95% ethanol content) ethanol solution (dissolve 30g of 95% ethanol into 500g of pure water), and heat at 45°C at the same time to make it Stir and dissolve for 6 minutes to obtain 560g peppermint oil and lemon essential oil solution;
[0063] 2) High-shear emulsification: ①first...
PUM
| Property | Measurement | Unit |
|---|---|---|
| length | aaaaa | aaaaa |
| width | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 