Preparation method of low-odor PVC building material decorative film
A low-odor, decorative film technology, applied in chemical instruments and methods, lamination auxiliary operations, lamination and other directions, can solve the problems of high odor and unpleasant taste of finished products, and achieve the effect of less environmental pollution, less harm and low odor
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] A preparation method of a low-odor PVC building material decorative film, comprising the steps of:
[0018] (1) Weigh the water-based printing ink according to the parts by mass: 10 parts of yellow, 20 parts of red, 5 parts of blue, 30 parts of gold oil, and 10 parts of water;
[0019] (2) Mix the above-mentioned printing ink raw materials and stir for 10 minutes at a speed of 100 rpm;
[0020] (3) Print the above-mentioned printing ink on the low-odor PVC tape base material through the printing machine, enter the oven at 50°C, and dry it for 5 seconds;
[0021] (4) Thermally bond the above-mentioned printed sample and low-odor PVC fabric in a small laminating machine at a bonding temperature of 150°C for 1 minute and a bonding pressure of 0.5Kg;
[0022] (5) After embossing and laminating the sample, after cooling for 3 minutes, the sample production is completed.
[0023] Wherein, the PVC tape base material in step (3) includes the following components in parts by m...
Embodiment 2
[0026] A preparation method of a low-odor PVC building material decorative film, comprising the steps of:
[0027] (1) Weigh the water-based printing ink according to the parts by mass: 30 parts of yellow, 40 parts of red, 15 parts of blue, 50 parts of gold oil, and 30 parts of water;
[0028] (2) Mix the above printing ink raw materials and stir for 20 minutes at a speed of 300 rpm;
[0029] (3) Print the above-mentioned printing ink on the low-odor PVC tape base material through the printing machine, enter the oven at 80°C, and dry it for 15 seconds;
[0030] (4) Thermally bond the above-mentioned printed samples and low-odor PVC fabrics on a small laminating machine at a bonding temperature of 200°C for 5 minutes and a bonding pressure of 1Kg;
[0031] (5) After embossing and laminating the sample, after cooling for 5 minutes, the sample production is completed.
[0032] Wherein, the PVC tape base material in step (3) includes the following components in parts by mass: 70...
Embodiment 3
[0035] A preparation method of a low-odor PVC building material decorative film, comprising the steps of:
[0036] (1) Weigh the water-based printing ink according to the parts by mass: 20 parts of yellow, 30 parts of red, 10 parts of blue, 40 parts of gold oil, and 20 parts of water;
[0037] (2) Mix the above-mentioned printing ink raw materials and stir for 15 minutes at a speed of 200 rpm;
[0038] (3) Print the above-mentioned printing ink on the low-odor PVC tape base material through the printing machine, enter the oven at 65°C, and dry it for 10 seconds;
[0039] (4) Thermally bond the above-mentioned printed samples and low-odor PVC fabrics in a small laminating machine at a bonding temperature of 170°C for 3 minutes and a bonding pressure of 0.7Kg;
[0040] (5) After embossing and laminating the sample, after cooling for 4 minutes, the sample production is completed.
[0041] Wherein, the PVC tape base material in step (3) includes the following components in parts...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com