Embodiment 1
[0035] The refining process of Eucommia crude glue comprises the following steps:
[0036] (1) send the eucommia thick glue solution through dissolving in the purifying kettle, then add flotation agent in the eucommia ulmoides thick glue solution through dissolving; mixture; the weight ratio of acrylic acid and acrylamide copolymer to glycerin is 2:1; the addition of the whole flotation agent is 0.05% of the weight of Eucommia crude glue;
[0037] (2) adopt the method for jacket heating to heat treatment to the material in the purification kettle in the step (1), the hot water temperature in the jacket is controlled at about 85 ℃, and the temperature of the material in the control step (1) remains at about 65 ℃ , and stir, the stirring speed is 400rpm;
[0038] (3) After stirring for 12 hours, settle for 5 hours, then separate the part containing impurities and flotation agent from the bottom, and repeat the cleaning of the upper clean glue solution several times according to...
Embodiment 2
[0041] The refining process of Eucommia crude glue comprises the following steps:
[0042] (1) The eucommia thick glue solution through dissolving is sent in the purifying kettle, then in the eucommia thick glue glue solution through dissolving, add flotation agent; Flotation agent is specifically the mixture of acrylic acid and acrylamide copolymer and pentylene glycol Mixture; the weight ratio of acrylic acid and acrylamide copolymer to pentylene glycol is 2:1; the addition of the entire flotation agent is 0.03% of the weight of Eucommia crude glue;
[0043] (2) adopt the method for jacket heating to material heat treatment in the purification still in step (1), the hot water temperature in the jacket is controlled at 80 ℃, the temperature of material in the control step (1) remains on 60 ℃, and Stirring, the stirring speed is 300rpm;
[0044] (3) After stirring for 1.5 hours, settle for 4 hours, then separate the part containing impurities and flotation agent from the bott...
Embodiment 3
[0046] The refining process of Eucommia crude glue comprises the following steps:
[0047] (1) Send the dissolved Eucommia coarse glue into the purification kettle, then add a flotation agent in the dissolved Eucommia coarse glue; the flotation agent is specifically acrylic acid and acrylamide copolymer and butylene glycol acetate A mixture of esters; the weight ratio of acrylic acid and acrylamide copolymer to butylene glycol acetate is 2:1; the addition of the entire flotation agent is 0.03% of the weight of Eucommia crude glue;
[0048] (2) adopt the method for jacket heating to material heat treatment in the purification still in step (1), the hot water temperature in the jacket is controlled at 80 ℃, the temperature of material in the control step (1) remains on 60 ℃, and Stirring, the stirring speed is 300rpm;
[0049] (3) After stirring for 1.5 hours, settle for 4 hours, then separate the part containing impurities and flotation agent from the bottom, and repeat the cl...