A degumming method and hemp fiber technology, which are applied in the chemical post-treatment of fibers, fiber treatment, textiles and papermaking, etc., can solve the problems of unsatisfactory degumming effect, affecting the processing quality of hemp fiber products and ramie fabrics, etc. The effect of removing and degumming is good, and the effect of reducing environmental pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] 1) Soda cooking
[0029] Get 50g of hemp fiber and place it in the boiling pot, add NaOH, NaOH and NaOH in the boiling pot 2 SiO 3 and detergent at 100°C for 60 minutes, the amount of NaOH is 5g / l, Na 2 SiO 3 The amount of detergent is 0.5g / l, and the amount of detergent is 0.5g / l;
[0030] 2) Washing and drying
[0031] Taking out the hemp fiber that has been boiled with alkali in the previous step, washing and drying to obtain anhydrous hemp fiber;
[0032] 3) Supercritical carbon dioxide fluid degumming
[0033] Place the anhydrous hemp fiber obtained in the previous step in a supercritical carbon dioxide fluid treatment device, first treat it at a pressure of 10MPa and a temperature of 115°C for 40 minutes, then treat it at a pressure of 29MPa and a temperature of 115°C for 40 minutes, and take it out for processing Post hemp fiber.
[0034] Tested according to GB5889-86, the cellulose content in the prepared fiber is 96.5%.
Embodiment 2
[0036] 1) Soda cooking
[0037] Get 50g of hemp fiber and place it in the boiling pot, add NaOH, NaOH and NaOH in the boiling pot 2 SiO 3 and detergent at 130°C for 40 minutes, the amount of NaOH is 5g / l, Na 2 SiO 3 The amount of detergent is 1g / l, and the amount of detergent is 2g / l;
[0038] 2) Washing and drying
[0039] Taking out the hemp fiber that has been boiled with alkali in the previous step, washing and drying to obtain anhydrous hemp fiber;
[0040] 3) Supercritical carbon dioxide fluid degumming
[0041] Place the anhydrous hemp fiber obtained in the previous step in a supercritical carbon dioxide fluid treatment device, first treat it at a pressure of 15MPa and a temperature of 80°C for 20 minutes, then treat it at a pressure of 29MPa and a temperature of 80°C for 20 minutes, and take it out for treatment Post hemp fiber.
[0042] Tested according to GB5889-86, the cellulose content in the prepared fiber is 97.5%.
Embodiment 3
[0044] 1) Soda cooking
[0045] Get 50g of hemp fiber and place it in the boiling pot, add NaOH, NaOH and NaOH in the boiling pot 2 SiO 3 and detergent at 170°C for 30 minutes, the amount of NaOH is 8g / l, Na 2 SiO 3 The amount of detergent is 1g / l, and the amount of detergent is 0.5g / l;
[0046] 2) Washing and drying
[0047] Taking out the hemp fiber that has been boiled with alkali in the previous step, washing and drying to obtain anhydrous hemp fiber;
[0048] 3) Supercritical carbon dioxide fluid degumming
[0049] Place the anhydrous hemp fiber obtained in the previous step in a supercritical carbon dioxide fluid treatment device, first treat it at a pressure of 10MPa and a temperature of 130°C for 60 minutes, then treat it at a pressure of 20MPa and a temperature of 130°C for 60 minutes, and take it out for treatment Post hemp fiber.
[0050] Tested according to GB5889-86, the cellulose content in the prepared fiber is 97.8%.
[0051] Embodiment 4, 5, 6, 7, 8 an...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com