Method for preparation of flame-proof chinlon gluing buckle
A manufacturing method and a technology for a hook and loop fastener are applied in the directions of fasteners, buckles, clothing, etc., which can solve the problems of flammability, hidden dangers of personal and vehicle safety, etc., and achieve the effect of improving safety and good flame retardant performance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0050] Example 1: Proceed as follows:
[0051] 1. Put the nylon hook and loop fastener into a four-corner tank dip dyeing machine in a roll shape, and clean it with a cleaning agent at 80°C for 30 minutes.
[0052] The formula of the cleaning agent is:
[0053] Nylon Velcro tape 200kg
[0054] Emulsifier LF100 1000g
[0055] PJ 400g
[0056] Water 3800kg
[0057] 2. Put the cleaned nylon hook and loop fastener into a continuous pad dyeing machine in a strip shape, and use a 60°C whitening finishing agent to whiten the nylon hook and loop fastener for 7 minutes. Coiled.
[0058] In the whitening finishing process, the formula of the whitening finishing agent is:
[0059] Nylon Velcro tape 200kg
[0060] Emulsifier LF-100 800g
[0061] PJ 100g
[0062] Fluorescent essence SP 7200cc
[0063] Acid Brilliant Blue A2R 2500cc
[0064] Glacial acetic acid HAC 600cc
[0065] Water softener EP-60 600cc
[0066] Water 3800kg
[0067] 3. Use an unwinding machine to untie the whitened nylon ho...
Embodiment 2
[0081] Example 2: Proceed as follows:
[0082] 1. Put the nylon hook and loop fastener into a common dip dyeing machine in a roll shape, and clean it with a 90°C cleaning agent for 20 minutes.
[0083] The formula of the cleaning agent is:
[0084] Nylon Velcro tape 200kg
[0085] Emulsifier LF100 900g
[0086] PJ 300g
[0087] Water 4000kg
[0088] 2. Put the cleaned nylon hook and loop fastener into the pad continuous dyeing machine in a strip shape, and use the whitening finishing agent at 80℃ to whiten the nylon hook and loop fastener for 6 minutes. Coiled.
[0089] In the whitening finishing process, the formula of the whitening finishing agent is:
[0090] Nylon Velcro tape 200kg
[0091] Emulsifier LF-100 900g
[0092] PJ 85g
[0093] Fluorescent essence SP 7000cc
[0094] Acid Brilliant Blue A2R 2200cc
[0095] Glacial acetic acid HAC 500cc
[0096] Water softener EP-60 500cc
[0097] Water 4000kg
[0098] 3. Use an unwinding machine to untie the whitened nylon hook and lo...
Embodiment 3
[0112] Example 3: Proceed as follows:
[0113] 1. Put the nylon hook and loop fastener into a common dip dyeing machine in a roll shape, and wash it with a 80℃ cleaning agent for 30 minutes.
[0114] The formula of the cleaning agent is:
[0115] Nylon Velcro tape 200kg
[0116] Emulsifier LF100 1000g
[0117] PJ 400g
[0118] Water 4300kg
[0119] 2. Put the cleaned nylon hook and loop fastener into a continuous pad dyeing machine in a strip shape, and use a 100 ℃ whitening finishing agent to whiten the nylon hook and loop fastener for 5 minutes. Coiled.
[0120] In the whitening finishing process, the formula of the whitening finishing agent is:
[0121] Nylon Velcro tape 200kg
[0122] Emulsifier LF-100 1000g
[0123] PJ 65g
[0124] Fluorescent essence SP 6500cc
[0125] Acid Brilliant Blue A2R 1200cc
[0126] Glacial acetic acid HAC 400cc
[0127] Water softener EP-60 400cc
[0128] Water 4300kg
[0129] 3. Use an unwinding machine to untie the whitened nylon hook and loop fa...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com