A kind of catalyst and its preparation method and application

A catalyst and application technology, applied in the field of catalyst preparation and decomposition of N2O, can solve the problems of low calcination temperature, industrial application, high decomposition temperature, low decomposition efficiency, etc., and achieve low decomposition temperature, high activity, high activity. Effect

Active Publication Date: 2014-10-22
BEIJING INSTITUTE OF PETROCHEMICAL TECHNOLOGY
View PDF7 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0010] Although some in the prior art described above have better activity, the calcination temperature is on the low side, and there is still a big gap from industrial application, and the decomposition temperature that has is higher, and the decomposition efficiency that has is low, and the carrier and active group The combination of points has not been reported

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0032] Weigh cobalt nitrate (Co(NO 3 ) 2 ·6H 2 O) 402.87g and citric acid (C 6 h 8 o 7 ·H 2 (O) 291.26g, respectively dissolved in water, prepared into a mixed aqueous solution, to obtain an aqueous solution containing metal salts and organic complexing agents, molecular sieve carrier HZSM-5 1000g was immersed in the aqueous solution, stirred continuously, and dried at a temperature of 70 ° C to make It is evenly loaded on the molecular sieve carrier to obtain the catalyst precursor, and then the precursor is roasted at 800 ° C for 6 hours to obtain the Co 3 o 4 / HZSM-5 catalyst, XRD analysis results show that the composite metal oxide has a spinel structure.

[0033] The catalyst is used for N 2 Decomposition of O, the gas composition is: 0.65v% N 2 O, 0.88v% O 2 , and the rest are N 2 Under the condition of N 2 O decomposition temperature T 10 330°C, T 95 It is 460°C.

[0034] The catalyst was subjected to an enhanced life experiment, and the experimental cond...

Embodiment 2

[0036] Take by weighing cobalt nitrate 181.55g and lanthanum nitrate (La(NO 3 ) 3 ·6H 2 (2) 540.26g and 393.76g of citric acid, are dissolved in water respectively, are mixed with mixed aqueous solution, obtain the aqueous solution containing metal salt and organic complexing agent, molecular sieve carrier HZSM-5 1000g inserts in the aqueous solution and impregnates, and constantly stirs, at 50 ℃ temperature drying, to obtain the catalyst precursor, and then the precursor was roasted at 500 ℃ for 8 hours to obtain the loading capacity of the present invention is 20% La 2 CoO 4 / HZSM-5 catalyst. XRD analysis results show that the composite metal oxide has a perovskite-like structure.

[0037] The catalyst is used for N 2 Decomposition of O, N 2 O decomposition temperature T 10 320°C, T 95 It is 472°C.

Embodiment 3

[0039] Take by weighing cobalt nitrate 516.00g and cerium nitrate (Ce(NO 3 ) 3 ·6H 2 (O) 769.90g and 746.09g of citric acid were respectively dissolved in water and prepared into a mixed aqueous solution to obtain an aqueous solution containing a metal salt and an organic complexing agent. Molecular sieve carrier RPSA 1000g was immersed in the aqueous solution and stirred continuously. Dry to obtain the catalyst precursor, and then roast the above precursor at 600°C for 5 hours to obtain the Co 1.5 Ce 1.5 o 4 / RPSA Catalyst. XRD analysis results show that the composite metal oxide has a spinel structure.

[0040] The catalyst is used for N 2 Decomposition of O, N 2 O decomposition temperature T 10 340°C, T 95 It is 440°C.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to a catalyst and a preparation method and application thereof. The catalyst contains a composite metal oxide and a molecular sieve carrier, wherein the composite metal oxide hasa spinel structure and / or a perovskite-like structure, and the molecular general formula of the composite metal oxide is Co3-xMxO4 or La2-yMyBO4. The molecular sieve carrier is an HZSM-5, HZSM-18 orRPSA molecular sieve with an MFI structure or an HY molecular sieve with a Y structure. The preparation method comprises the following steps: dissolving a corresponding metal salt and a correspondingorganic complexing agent into water respectively; putting the carrier into the aqueous solution for soaking; drying the mixture at a temperature of between 30 and 90 DEG C to obtain a catalyst precursor; and calcinating the catalyst precursor at a temperature of between 400 and 1,000 DEG C for 2 to 10 hours to obtain the catalyst. The catalyst has high activity and good stability; the decomposition temperature of N2O is low; after strengthening experiments for 100 hours, the catalyst still has high activity; and the analysis result of a scanning electron microscope shows that the surface shapeof the catalyst is basically not changed.

Description

technical field [0001] The invention relates to a catalyst used in air pollution control technology, in particular to a catalyst for decomposing N 2 O catalyst. [0002] The invention also relates to the preparation method and application of the catalyst. Background technique [0003] N 2 O is an important air pollutant, which is not only a greenhouse gas, but also has a destructive effect on the ozone layer. N 2 The greenhouse effect of O is respectively that of CO 2 310 times of CH 4 21 times of (Ram rez J P, Kapteijn F, Fel K, et al. Formation and control of N 2 O in nitric acid production. Where do we stand today? [J]. Appl. Catal. B, 2003, 44: 1). N 2 Sources of O come from the oceans, land, agriculture, combustion processes of various fossil fuels and the chemical industry. Nitric acid plants and nitric acid oxidation processes, such as organic synthesis plants producing adipic acid and glyoxal are N 2 The largest emission source of O. With the contin...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): B01J29/064B01J29/40B01J29/08B01J37/03B01D53/56
CPCY02C20/10
Inventor王虹李翠清宋永吉王军利迟姚玲
OwnerBEIJING INSTITUTE OF PETROCHEMICAL TECHNOLOGY