Embodiment 1
[0030] Embodiment 1: A method for manufacturing an anti-corrugated interlining, comprising the following process steps:
[0031] (1) Preparation of base fabric: choose polyester fabric with broken twill weave method, 30d×30d;
[0032] (2) Scouring: Add water and 2.0 g / L desizing agent into the liquid tank of the scouring machine to prepare a scouring liquid with a bath ratio of 26:1; after the temperature rises to 50°C, put the base fabric into the liquid tank to make The scouring liquid and the base cloth circulate in the liquid cylinder for 10 minutes; then heat up to a scouring temperature of 80°C, after 60 minutes of scouring, drain the refining liquid, add cold water to wash, and take out the base cloth;
[0033] (3) Finishing: Add water, 1.5 g / L waterproofing agent, 0.2 g / L antistatic agent and 4 g / L fluffing agent into the liquid tank of the finishing machine to make a finishing liquid, so that the base fabric can be dipped and rolled Finishing solution, the excess rat...
Embodiment 2
[0035] Embodiment 2: A method of manufacturing anti-corrugated interlining, comprising the following process steps:
[0036] (1) Base fabric preparation: choose polyester fabric with broken twill weave 30d×30d;
[0037](2) Scouring: Add water and 4.0 g / L desizing agent into the liquid tank of the scouring machine to prepare a scouring liquid with a liquor ratio of 29:1; after the temperature rises to 70°C, put the base fabric into the liquid tank to make The scouring liquid and the base cloth are circulated in the liquid cylinder for 5 minutes; then the temperature is raised to scouring temperature 100°C, after 30 minutes of scouring, the refining liquid is drained, and the base cloth is taken out after washing with cold water;
[0038] (3) Finishing: Add water, 2.5 g / L waterproofing agent, 0.5 g / L antistatic agent and 6 g / L fluffing agent into the liquid tank of the finishing machine to make a finishing liquid, so that the base fabric can be dipped and rolled Finishing solut...
Embodiment 3
[0043] Embodiment 3: The manufacturing method of anti-corrugated interlining comprises the following process steps:
[0044] (1) Base fabric preparation: choose polyester fabric with broken twill weave 30d×30d;
[0045] (2) Scouring: Add water and 3 g / L desizing agent into the liquid tank of the scouring machine to prepare a scouring liquid with a liquor ratio of 27:1; after the temperature rises to 60°C, put the base fabric into the liquid tank to make The scouring liquid and the base cloth circulate in the liquid cylinder for 8 minutes; then heat up to the scouring temperature of 90°C, after 45 minutes of scouring, drain the refining liquid, add cold water to wash, and take out the base cloth;
[0046] (3) Finishing: Add water, 2 g / L waterproofing agent, 0.3 g / L antistatic agent and 5 g / L bulking agent into the liquid tank of the finishing machine to make a finishing liquid, so that the base fabric can be dipped and rolled Finishing solution, the excess rate is 60%; then th...