Embodiment 1
[0033] This embodiment provides a gradient anodic oxidation method to prepare a gradient-wettable hydrophilic-hydrophobic interphase copper surface with a relatively large hydrophilic region area ratio. The specific steps are:
[0034] The first step, the preparation of electrolyte:
[0035] Weigh 1g of sodium hydroxide particles, dissolve in 500g of deionized water, and stir until completely dissolved.
[0036] The second step, target sample surface pretreatment:
[0037] Cut the copper sheet into a rectangle with a length of 3.5cm and a width of 1.5cm, soak it in dilute hydrochloric acid for 15 minutes, then ultrasonically clean it with ethanol and water for 20 minutes, and dry it in a drying oven at 70°C for 10 minutes stand-by.
[0038] The third step is to prepare gradient wettable hydrophilic-hydrophobic interphase surface by anodic oxidation method:
[0039] First, one side of the target sample is closely attached to the insulating porous mask. The hole diameter of t...
Embodiment 2
[0043] This embodiment provides a method for preparing a gradient-wettable hydrophilic-hydrophobic interphase copper surface with a smaller hydrophilic region area ratio by gradient anodic oxidation. The specific steps are:
[0044] The first step, the preparation of electrolyte:
[0045] Weigh 1g of sodium hydroxide particles, dissolve in 500g of deionized water, and stir until completely dissolved.
[0046] The second step, target sample surface pretreatment:
[0047] Cut the copper sheet into a rectangle with a length of 3.5cm and a width of 1.5cm, soak it in dilute hydrochloric acid for 15 minutes, then ultrasonically clean it with ethanol and water for 20 minutes, and dry it in a drying oven at 70°C for 10 minutes stand-by.
[0048] The third step is to prepare gradient wettable hydrophilic-hydrophobic interphase surface by anodic oxidation method:
[0049] First, one side of the target sample is closely attached to the insulating porous mask. The hole diameter of the ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com