Infrared jade wallpaper
An infrared and wallpaper technology, applied in paper, papermaking, paper coating and other directions, can solve problems such as affecting people's health, harmful gases and bacteria producing odor, etc., to achieve the effect of benefiting health, removing odor and protecting health
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] Embodiment 1: Infrared jade wallpaper, the wallpaper slurry is configured by the following components according to the mass percentage content:
[0029] Main resin 70%;
[0030] Thickener 1%;
[0031] Dispersant 3%;
[0032] Illite powder 10%;
[0033] Jade powder 8%;
[0034] The balance is water.
[0035] The preparation process of wallpaper is:
[0036] a. Mixing: After the wallpaper slurry is prepared, mix it evenly;
[0037] b. Material preparation: apply wallpaper slurry to the paper base layer, and then emboss it through a pressure roller to form a wallpaper blank;
[0038] c. Drying: Dry the wallpaper base at high temperature;
[0039] d. Winding: After drying, it is cured at room temperature and then rolled to obtain environmentally friendly absorbent wallpaper.
[0040] The drying temperature is 150°C.
[0041] The curing time is 3 minutes.
[0042] The fineness of illite powder is 1.6.
[0043] Jade powder is a mixed powder of white marble jade pow...
Embodiment 2
[0047] Embodiment 2: Infrared jade wallpaper, the wallpaper slurry is configured by the following components according to the mass percentage content:
[0048] Main resin 80%;
[0049] Thickener 1%;
[0050] Dispersant 1%;
[0051] Illite powder 10%;
[0052] Jade powder 3%;
[0053] The balance is water.
[0054] The preparation process of wallpaper is:
[0055] a. Mixing: After the wallpaper slurry is prepared, mix it evenly;
[0056] b. Material preparation: apply wallpaper slurry to the paper base layer, and then emboss it through a pressure roller to form a wallpaper blank;
[0057] c. Drying: Dry the wallpaper base at high temperature;
[0058] d. Winding: After drying, it is cured at room temperature and then rolled to obtain environmentally friendly absorbent wallpaper.
[0059] The drying temperature is 180°C.
[0060] The curing time is 5 minutes.
[0061] The fineness of illite powder is 1.0.
[0062] Jade powder is a mixed powder of white marble jade pow...
Embodiment 3
[0066] Embodiment 3: Infrared jade wallpaper, the wallpaper slurry is configured according to the mass percentage content of the following components:
[0067] Main resin 85%;
[0068] Thickener 1%;
[0069] Dispersant 2%;
[0070] Illite powder 8%;
[0071] Jade powder 3%;
[0072] The balance is water.
[0073] The preparation process of wallpaper is:
[0074] a. Mixing: After the wallpaper slurry is prepared, mix it evenly;
[0075] b. Material preparation: apply wallpaper slurry to the paper base layer, and then emboss it through a pressure roller to form a wallpaper blank;
[0076] c. Drying: Dry the wallpaper base at high temperature;
[0077] d. Winding: After drying, it is cured at room temperature and then rolled to obtain environmentally friendly absorbent wallpaper.
[0078] The drying temperature is 200°C.
[0079] The curing time is 5 minutes.
[0080] The fineness of illite powder is 1.6.
[0081] Jade powder is a mixed powder of white marble jade powd...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com