Preparation technology and application of a new imprinted material of composite metal polyphenols co-complex
A technology for compounding metals and imprinting materials, which can be applied in other chemical processes, chemical instruments and methods, etc., can solve the problems of low selection and recognition ability and application limitations, and achieve the effect of high imprinting efficiency, strong selectivity and improved purity of materials.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] (1) Weigh Tb(NO 3 ) 3 ·6H 2 O and MnSO 4 , dissolved in 100mL deionized water, slowly drop NaOH solution while stirring, until the pH is 8.5-11, stir, age at room temperature for 5-8h, filter, wash the precipitate with deionized water until neutral, at 60°C Dry for 24 hours and set aside;
[0017] (2) Add 0.5-1.0 mmol of chlorogenic acid-caffeic acid-vanillic acid-protocatechuic acid mixture in a molar ratio of 1:2:2:1, 0.4 mL dimethyl sulfoxide (DMSO), 6.0mL of acetonitrile-tetrahydrofuran mixed solvent (volume ratio 1:2), ultrasonically mixed, slightly heated, and 1.2g of the precipitate obtained in step (1) and 2.0mL of additives (0.34mol / L HF- NaF buffer solution), stirred and allowed to stand for 2-3h to obtain a composite metal-polyphenol complex solution;
[0018] (3) Add 1.6 mmol of acrylamide-dopamine mixed functional monomer (molar ratio 1:8) to the solution obtained in step (2), sonicate for 10 minutes, then add 9 mg of azobisisobutyronitrile (AIBN), and...
Embodiment 2
[0022] (1) Weigh Tb(NO 3 ) 3 ·6H 2 O and MnSO 4 , dissolved in 100mL deionized water, slowly drop NaOH solution while stirring, until the pH is 8.5-11, stir, age at room temperature for 5-8h, filter, wash the precipitate with deionized water until neutral, at 60°C Dry for 24 hours and set aside;
[0023] (2) Add 0.5-1.0 mmol of chlorogenic acid-caffeic acid-vanillic acid-protocatechuic acid mixture in a molar ratio of 1:2:2:1, 0.4 mL dimethyl sulfoxide (DMSO), 6.0mL of acetonitrile-tetrahydrofuran mixed solvent (volume ratio 1:2), ultrasonically mixed, slightly heated, 1.5g of the precipitate obtained in step (1) and 1.7mL of auxiliary ingredients (0.34mol / L HF- NaF buffer solution), stirred and allowed to stand for 2-3h to obtain a composite metal-polyphenol complex solution;
[0024] (3) Add 1.6 mmol of acrylamide-dopamine mixed functional monomer (molar ratio 1:9) to the solution obtained in step (2), sonicate for 10 minutes, then add 9 mg of azobisisobutyronitrile (AI...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com