High-quality peeling method for wickerwork raw materials
A high-quality, raw material technology, applied in the fields of wicker bar peeling, mechanical equipment, etc., can solve the problems of unsatisfactory peeling machine effect, large time and labor consumption, and high cost, so as to achieve great market competitiveness and promotion and application value , Improve efficiency and effect, and achieve high separation efficiency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] A high-quality peeling method for wicker raw materials, comprising the steps of:
[0020] (1) Alkaline soaking treatment:
[0021] After bundling the wicker raw materials into bundles, put them into the pool, then put 0.1% quicklime into the pool water, stir for 15 minutes, and take out the bundled wicker raw materials for later use;
[0022] (2) Freezing treatment:
[0023] Put the bundled willow weaving raw materials processed in step (1) into the freezer for freezing treatment, and take them out after 6 hours for later use;
[0024] (3) Ultrasonic treatment:
[0025] Ultrasonic treatment is performed on the wicker raw material treated in step (2), and peeling of the wicker raw material is done after 2 hours.
[0026] Further, the stirring speed during the stirring treatment in step (1) is 100 rpm.
[0027] Further, during the freezing treatment described in step (2), the temperature in the freezing chamber is controlled to be -8°C.
[0028] Further, the frequenc...
Embodiment 2
[0030] A high-quality peeling method for wicker raw materials, comprising the steps of:
[0031] (1) Alkaline soaking treatment:
[0032] After bundling the willow weaving raw materials into bundles, put them into the pool, then put 0.2% quicklime in the pool water into the pool, stir for 18 minutes, and take out the bundled willow weaving raw materials for later use;
[0033] (2) Freezing treatment:
[0034] Put the bundled willow weaving raw materials processed in step (1) into the freezer for freezing treatment, and take them out after 7 hours for later use;
[0035] (3) Ultrasonic treatment:
[0036] Ultrasonic treatment is performed on the wicker raw material treated in step (2), and peeling of the wicker raw material is done after 2.5 hours.
[0037] Further, the stirring speed during the stirring treatment in step (1) is 130 rpm.
[0038] Further, during the freezing treatment in step (2), the temperature in the freezing chamber is controlled to be -9°C.
[0039] F...
Embodiment 3
[0041] A high-quality peeling method for wicker raw materials, comprising the steps of:
[0042] (1) Alkaline soaking treatment:
[0043] After bundling the willow weaving raw materials into bundles, put them into the pool, then put 0.3% quicklime into the pool water, mix them for 20 minutes, and take out the bundled willow weaving raw materials for later use;
[0044] (2) Freezing treatment:
[0045] Put the bundled willow weaving raw materials processed in step (1) into the freezer for freezing treatment, and take them out after 8 hours for later use;
[0046] (3) Ultrasonic treatment:
[0047] Ultrasonic treatment is performed on the wicker raw material treated in step (2), and peeling of the wicker raw material is done after 3 hours.
[0048] Further, the stirring speed during the stirring treatment in step (1) is 150 rpm.
[0049] Further, during the freezing treatment in step (2), the temperature in the freezing chamber is controlled to be -10°C.
[0050] Further, t...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com