Water-based anti-yellowing whitening paint curtain-coating process

A technology of yellowing resistance and white paint, applied in the field of paint technology, can solve the problems of surface paint peeling, paint discoloration, moldy plates, etc.

Inactive Publication Date: 2020-08-25
MENGTIAN HOUSEHOLD GRP CO LTD
View PDF1 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002] Now there are more and more types of paints on the market, and more and more functions, but in the process of use, there are mixed reviews. The problem is often not the paint itself, but the painting process, the common painting process , although the method is simple, the use effect is very poor. With the growth of time, problems such as mildew inside the board, peeling off of the surface paint, and discoloration of the paint will also appear.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0033] S1. The first white-ground flow coating: use a flow coater and water-based anti-yellowing white paint to carry out the first white-ground flow coating on the wooden door, and the coating amount of the water-based anti-yellowing white paint is 60g / ㎡;

[0034] S2. Surface dry: Surface dry for 30 minutes in an environment with a temperature of 30°C and a humidity of 30%;

[0035] S3. The second white-ground flow coating: use a flow coating machine and water-based anti-yellowing white paint to carry out the second white-ground flow coating on the wooden door, and the coating amount is 60g / ㎡;

[0036] S4. Drying: surface dry for 60 minutes in an environment with a temperature of 30°C and a humidity of 30%; then pull it into a drying tunnel and dry it in a drying tunnel at a temperature of 45°C for 180 minutes;

[0037] S5. Sandblasting: use a sander to perform sandblasting on the dried wooden door;

[0038] S6. The first pass of white surface coating: use a flow coating mac...

Embodiment 2

[0043] S1. The first white-ground flow coating: use a flow coater and water-based anti-yellowing white paint to carry out the first white-ground flow coating on wooden doors, and the coating amount of water-based yellowing-resistant white paint is 65g / ㎡;

[0044] S2. Surface dry: Surface dry for 30 minutes in an environment with a temperature of 35°C and a humidity of 50%;

[0045] S3. The second white-ground flow coating: use a flow coating machine and water-based anti-yellowing white paint to carry out the second white-ground flow coating on the wooden door, and the coating amount is 65g / ㎡;

[0046] S4. Drying: surface dry for 60 minutes in an environment with a temperature of 35°C and a humidity of 50%; then pull it into a drying tunnel and dry it in a drying tunnel at a temperature of 52.5°C for 180 minutes;

[0047] S5. Sandblasting: use a sander to perform sandblasting on the dried wooden door;

[0048] S6. The first pass of white surface coating: use a flow coating mac...

Embodiment 3

[0053] S1. The first white-ground flow coating: use a flow coating machine and water-based anti-yellowing white paint to carry out the first white-ground flow coating on wooden doors, and the coating amount of water-based yellowing-resistant white paint is 70g / ㎡;

[0054] S2. Surface dry: Surface dry for 30 minutes in an environment with a temperature of 40°C and a humidity of 70%;

[0055] S3. The second white-ground flow coating: use a flow coating machine and water-based anti-yellowing white paint to carry out the second white-ground flow coating on the wooden door, and the coating amount is 70g / ㎡;

[0056] S4. Drying: surface dry for 60 minutes in an environment with a temperature of 40°C and a humidity of 70%; then pull it into a drying tunnel and dry it in a drying tunnel at a temperature of 60°C for 180 minutes;

[0057] S5. Sandblasting: use a sander to perform sandblasting on the dried wooden door;

[0058] S6. The first pass of white surface coating: use a flow coat...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a water-based anti-yellowing whitening paint curtain-coating process. The process comprises the following steps that the first time of white primer curtain-coating on a woodendoor is conducted by using a curtain coater and water-based anti-yellowing whitening paint, and the second time of white primer curtain-coating is conducted after surface drying, specifically, surfacedrying is conducted for 60 minutes under the temperature of 30-40 DEG C and the humidity of 30% to 70%; then the wooden door is pulled into a drying channel and dried for 180 minutes in the drying channel with the temperature of 45-60 DEG C; then the dried wooden door is subjected to slinging operation by using a sander; the first time of white finishing coat curtain-coating is conducted, and surface drying is conducted for 30 minutes under the temperature of 30-40 DEG C and the humidity of 30% to 70% after surface drying; then the second time of water-finishing coat curtain-coating is conducted, specifically, the surface drying is conducted for 60 minutes under the temperature of 30-40 DEG C and the humidity of 30% to 70%; and the wooden door is pulled into the drying channel and dried for 180 minutes in the drying channel with the temperature of 45-60 DEG C.

Description

technical field [0001] The invention relates to the field of paint technology, in particular to a water-based anti-yellowing white paint flow coating process. Background technique [0002] Nowadays, there are more and more types of paints on the market, and there are more and more functions, but in the process of use, there are mixed opinions. The problem is often not the paint itself, but the painting process, the common painting process , although the method is simple, the use effect is very poor. As time goes by, problems such as mildew inside the board, peeling off of the surface paint, and discoloration of the paint will also appear. Contents of the invention [0003] The purpose of the present invention is to address the deficiencies in the prior art and provide a water-based anti-yellowing white paint flow coating process to solve the problems in the prior art. [0004] The technical problem solved by the present invention can adopt following technical scheme to re...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): B05D7/24
CPCB05D7/24B05D7/584
Inventor 余静渊周学良崔正峰唐其徐学峰
Owner MENGTIAN HOUSEHOLD GRP CO LTD