Asphalt composition and preparation method thereof

A bitumen composition and bitumen technology, which are applied in building structures, buildings, building components, etc., can solve the problems of losing the bitumen export market, failing to meet the requirements of bitumen quality indicators, and failing to export bitumen products, and achieving a simple and easy production process. The effect of obtaining and enhancing export competitiveness

Active Publication Date: 2022-05-03
CHINA PETROLEUM & CHEM CORP
View PDF10 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, the asphalt quality indicators in foreign countries are quite different from those in my country. It is difficult for asphalt products produced by using our traditional petroleum refining raw materials, formulas and processes to meet the quality standards of foreign asphalt.
[0003] For example, although the annual import demand of asphalt products in Australia is as high as one million tons, the asphalt products produced by my country's traditional petroleum refining raw materials and production process formula are mainly All of them meet the domestic asphalt product standards, but cannot meet the Australian asphalt quality index requirements, so the asphalt products produced cannot be exported to Australia, and an important asphalt export market has been lost in vain.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Asphalt composition and preparation method thereof
  • Asphalt composition and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0086] (1) After heating 76 parts by mass of vacuum residue to a temperature of 145° C., put it into an asphalt mixing tank, and perform mechanical stirring at a temperature of 145° C.

[0087] (2) Add 4 parts by mass of light blended oil into an asphalt blending tank and perform mechanical stirring and blending with vacuum residue at a temperature of 145°C for 4 hours.

[0088] (3) Cool down the prepared mixture to 135°C and keep the temperature stable for 1 hour.

[0089] (4) Add 20 parts by mass of heavy blending oil into an asphalt blending tank and directly perform mechanical stirring with the mixture in step (3) at a temperature of 135° C. for 3 hours to obtain the finished product.

[0090] (5) After the mixing and blending is completed, the finished product is put into an asphalt storage tank for storage at a storage temperature of 120°C, and must be shipped within 15 days of storage.

[0091] The vacuum residue in this example is a vacuum residue product produced by ...

Embodiment 2

[0099] (1) After heating 72 parts by mass of vacuum residue to a temperature of 150° C., put it into an asphalt mixing tank, and perform mechanical stirring at a temperature of 150° C.

[0100] (2) Add 5 parts by mass of light blended oil into an asphalt blending tank and perform mechanical stirring and blending with vacuum residual oil at a temperature of 150° C. for 5 hours.

[0101] (3) Cool down the prepared mixture to 140°C and keep the temperature stable for 2 hours.

[0102] (4) Add 23 parts by mass of heavy blending oil into an asphalt blending tank and directly perform mechanical stirring with the mixture in step (3) at a temperature of 140° C. for 4 hours to obtain the finished product.

[0103] (5) After the mixing and blending is completed, the finished product is put into an asphalt storage tank for storage at a storage temperature of 110°C, and must be shipped within 15 days of storage.

[0104] The vacuum residue in this example is produced by mixing Ecuadorian...

Embodiment 3

[0113] (1) After heating 80 parts by mass of vacuum residue to a temperature of 140°C, put it into an asphalt mixing tank, and perform mechanical stirring at a temperature of 140°C.

[0114] (2) Add 3 parts by mass of light blended oil into an asphalt blending tank and perform mechanical stirring and blending with vacuum residue at a temperature of 140°C for 4 hours.

[0115] (3) Cool down the prepared mixture to 130°C and keep the temperature stable for 1 hour.

[0116] (4) Add 17 parts by mass of heavy blending oil into an asphalt blending tank and directly perform mechanical stirring with the mixture in step (3) at a temperature of 130° C. for 3 hours to obtain the finished product.

[0117] (5) After the mixing and blending is completed, the finished product is put into an asphalt storage tank for storage at a storage temperature of 120°C, and must be shipped within 15 days of storage.

[0118] The vacuum residue in this example is a vacuum residue product produced by mix...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
flash pointaaaaaaaaaa
densityaaaaaaaaaa
densityaaaaaaaaaa
Login to View More

Abstract

The invention relates to an asphalt composition and a preparation method thereof. The asphalt composition is prepared from the following components in parts by weight: 69 to 83 parts of vacuum residue, 15 to 25 parts of heavy blended oil and 2 to 6 parts of light blended oil. The vacuum residual oil is produced by adopting specific and appropriate crude oil, a specific mixing ratio and a specific production process, and then the vacuum residual oil, the light blended oil and the heavy blended oil which meet specific requirements are stirred and blended according to a specified ratio to produce an asphalt product which meets the quality index requirements of Australian C-170 exported asphalt. The problem that asphalt products produced by adopting traditional petroleum refining raw materials, formulas and processes in China cannot reach export asphalt quality indexes is solved.

Description

technical field [0001] The invention belongs to the technical field of oil refining and chemical materials, and in particular relates to an asphalt composition and a preparation method thereof. Background technique [0002] In recent years, with the increasing oil refining capacity of domestic refineries, domestic asphalt production capacity has also increased rapidly, resulting in fierce competition in the domestic asphalt product market, especially homogeneous competition. In order to seek higher profits and sales, domestic oil refiners hope to produce asphalt products that meet foreign standards. However, there is a big difference between foreign asphalt quality indicators and our country's asphalt quality indicators. It is difficult for asphalt products produced by our traditional petroleum refining raw materials, formulas and processes to meet foreign asphalt quality standards. [0003] For example, although Australia’s annual import demand for asphalt products is as h...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C08L95/00C08L91/00
CPCC08L95/00C08L2205/025C08L2205/035C08L91/00Y02A30/30
Inventor 何靖斌谭达刚黄艳芳欧晔梁红梅苏亦平
Owner CHINA PETROLEUM & CHEM CORP