[0022] 1. Preparation of inkjet printing pigment ink:
[0023] Take 25g of pigment red paste, 10g of diethylene glycol, 5g of glycerol, 20g of adhesive HY-FB, 10g of water-based polyurethane, 5g of citric acid, 0.3g of OP-10, and 24.7g of deionized water. Put the above components into the container in turn, mix evenly, stir with a mixer at 450 rpm for 10 minutes, filter (0.5 μm microporous membrane) to make superfine pigment red ink;
[0024] 2. Inkjet printing:
[0025] Use the inkjet printing machine to print the superfine pigment red ink on the pure cotton woven calico, dry it in the oven under the condition of temperature: 80°C, time: 3 minutes, and then at the temperature: 150°C , the time is: bake and fix the color under the condition of 3 minutes. Obtain sample A, and test the color fastness of the fabric using a rubbing fastness meter and a color measuring and matching instrument. The results are shown in Table 1.
Embodiment 2
[0027] 1. Preparation of inkjet printing pigment ink:
[0028] Get pigment yellow paste 15g, diethylene glycol 15g, polyethylene glycol 200 10g, 1,4-butanediol 10g, glycerol 5g, binder FWT (BASF company) 10g, crosslinking agent EH 5g , butane tetracarboxylic acid 10g, Pingpingjia 0 0.5g, Tween 80 0.5g, deionized water 19g. Put the above components into the container in turn, mix evenly, stir with a mixer at 500 rpm for 15 minutes, filter (0.5 μm microporous membrane) to make superfine pigment yellow ink;
[0029] 2. Inkjet printing:
[0030] Use the inkjet printing machine to print the superfine pigment yellow ink on the pure cotton woven calico, dry it in the oven under the condition of temperature: 90°C, time: 2 minutes, and then at the temperature: 140°C , the time is baked and fixed under the condition of 4 minutes. Obtain sample B, and test the color fastness of the fabric by using a rubbing fastness meter and a color measuring and matching instrument. The results are...
Embodiment 3
[0032] 1. Preparation of inkjet printing pigment ink:
[0033] Get 15g of pigment blue paste, 1,4-butanediol 10g, glycerol 15g, binder HY-FB (Qingdao Haiyi Company) 20g, butane tetracarboxylic acid 10g, Tween 60 0.5g, deionized Water 29.5g. Put the above components into the container in turn, mix evenly, stir with a mixer at 550 rpm for 12 minutes, filter (0.5 μm microporous membrane) to make ultrafine pigment blue ink;
[0034] 2. Inkjet printing:
[0035] Use the inkjet printing machine to print the ultra-fine pigment blue ink on the pure cotton woven calico, dry it in the oven at a temperature of 85°C and a time of 4 minutes, and then dry it at a temperature of 135°C , the time is baked and fixed under the condition of 3.5 minutes. Obtain sample C, and test the color fastness of the fabric by using a rubbing fastness meter and a color measuring and matching instrument. The results are shown in Table 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com