Low-alloy bainite ductile iron oil quenching isothermal tempering heat treatment process

A technology of bainitic ductile graphite and isothermal tempering, which is applied in the field of metal materials and ductile iron, can solve the problems affecting the structure and material properties of ductile iron, the reduction of material strength, hardness and toughness, and the inability to effectively control the heat preservation temperature. Achieve the effects of reducing equipment investment, good wear resistance, and good impact toughness

Inactive Publication Date: 2008-06-18
GUILIN UNIV OF ELECTRONIC TECH
View PDF1 Cites 4 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The isothermal furnace cannot effectively control the holding temperature, which affects the structure and material properties of ductile iron. The residual austenite in the structure increases, and even pearlite transformation occurs. Therefore, when the size of the part is large, the depth of the hardened layer cannot reach Requirements, so that the internal strength, hardness and toughness of the material will be significantly reduced

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0023] Green sand molding, melting alloys in a one-ton cupola.

[0024] (1) Metal charge: high-quality No. 18 Benxi pig iron, returned furnace iron, ferromolybdenum, ferrosilicon, ferromanganese, scrap copper, scrap steel, returned furnace charge and spheroidized alloy. The chemical composition requirements of ductile iron are as follows (mass percentage):

[0025] C: 3.60 S i : 2.80 Mn: 0.15 Cr: 0.18

[0026] Mo: 0.35 S: 0.02 P: 0.07 Mg: 0.05

[0027] Cu: 0.50 Bi: 0.02R e : 0.05F e :margin.

[0028] (2) Melting of molten iron: put pig iron, scrap steel, and returned materials into the furnace in batches according to requirements for melting, and add them after the ferroalloy furnace, and control the tapping temperature at 1420-1450 °C.

[0029] (3) Spheroidizing treatment: the spheroidizing agent is made of rare earth magnesium-silicon alloy, the dosage is 1.6% of the molten iron, the particle size is 10-20mm (range), and it is treated by the flushing method.

[0030] ...

Embodiment 2

[0037] Green sand molding, melting alloys in a one-ton cupola.

[0038] (1) Metal charge: high-quality No. 18 Benxi pig iron, returned furnace iron, ferromolybdenum, ferrosilicon, ferromanganese, scrap copper, scrap steel, returned furnace charge and spheroidized alloy. The chemical composition requirements of ductile iron are as follows (mass percentage):

[0039] C: 3.56S i : 3.2 Mn: 0.15 Cr: 0.20

[0040] Mo: 0.35 S: 0.02 P: 0.07 Mg: 0.05

[0041] Cu: 0.50 Bi: 0.02R e : 0.05F e :margin.

[0042] (2) Melting of molten iron: put pig iron, scrap steel, and returned materials into the furnace in batches according to requirements for melting, and add them after the ferroalloy furnace, and control the tapping temperature at 1420-1450 °C.

[0043] (3) Spheroidizing treatment: the spheroidizing agent is made of rare earth magnesium-silicon alloy, the dosage is 1.6% of the molten iron, the particle size is 10-20mm (range), and it is treated by the flushing method.

[0044] (4...

Embodiment 3

[0050] Green sand molding, melting alloys in a one-ton cupola.

[0051] (1) Metal charge: high-quality No. 18 Benxi pig iron, returned furnace iron, ferromolybdenum, ferrosilicon, ferromanganese, scrap copper, scrap steel, returned furnace charge and spheroidized alloy. The chemical composition requirements of ductile iron are as follows (mass percentage):

[0052] C: 3.62S i : 3.5 Mn: 0.15 Cr: 0.19

[0053] Mo: 0.40 S: 0.02 P: 0.07 Mg: 0.05

[0054] Cu: 0.50 Bi: 0.03 R e : 0.05F e :margin.

[0055] (2) Melting of molten iron: put pig iron, scrap steel, and returned materials into the furnace in batches according to requirements for melting, and add them after the ferroalloy furnace, and control the tapping temperature at 1420-1450 °C.

[0056] (3) Spheroidizing treatment: the spheroidizing agent is made of rare earth magnesium-silicon alloy, the dosage is 1.6% of the molten iron, the particle size is 10-20mm (range), and it is treated by the flushing method.

[0057] (...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
thicknessaaaaaaaaaa
thicknessaaaaaaaaaa
thicknessaaaaaaaaaa
Login to view more

Abstract

A low alloy bainite ductile iron oil quenching with temperature isothermal tempering heat treatment process includes: (1) heating a ductile iron work piece to be at 880 to 960 DEG C for the austenization; (2) quenching the work piece in machine oil; (3) taking out the ductile iron work piece when the surface temperature is 150 to 230 DEG C; (4) keeping the ductile iron work piece with temperature and rapidly burying sands for the heat preservation and the tempering for 6 to 8 hours; or burying sands for the heat preservation and the tempering for 1 to 3 hours and then taking the work piece out for the air cooling. Through refractory bricks and molding sands in an insulation packet or a ground pit, the process forms a reasonable temperature gradient from the inside of the ductile iron to the surface, a sands layer, the insulation packet or the ground pit. The slow and stable cooling speed which accords with the requirement is established. The isothermal tempering temperature is effectively controlled. The residue heat after the heat treatment on the ductile iron work piece is used to realize the isothermal transformation from austenite to bainite, which is more beneficial to the formation of bainite tissues. The obtained ductile iron work piece tissues have the advantages of reasonable structure and perfect comprehensive property and are especially applied to gears, crankshafts, grinding balls, etc.

Description

Technical field: [0001] The present invention relates to metallic materials, particularly ductile iron, more particularly low alloy bainitic ductile iron. Background technique: [0002] Low-alloy bainitic ductile iron has high strength, hardness and toughness, and has good casting performance. It is known as one of the major achievements in cast iron metallurgy in the past 40 years. At present, the heat treatment methods for obtaining bainite ductile iron mainly include traditional salt bath isothermal cooling and water medium cooling to control isothermal quenching (CN200510044091.X). Wei Deqiang's "Research and Production of Bainitic Nodular Cast Iron Grinding Ball Material" (Journal of Xiangtan University of Science and Technology 2005.Vol.27No.1: 94-97), discloses the production of heat treatment process using casting waste heat step-by-step isothermal quenching (oil quenching) Low alloy (Mo, M n 、C u 、C r ) The method of ductile iron grinding ball material, using 90...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C21D1/18C21D9/36
Inventor 魏德强王荣
Owner GUILIN UNIV OF ELECTRONIC TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products