Russian fat coal participant coking and coal blending method
A technology for coking coal and fat coal, which is applied in coke ovens, petroleum industry, etc., can solve problems such as a large amount of foamed coke and deteriorated coke quality, and achieve the effect of reducing the cost of coal blending
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] Russian fat coal participates in the method of coking coal blending, which includes the steps of mixing individual coking coals. The raw material components and weight percentages of the single coking coals used are:
[0027] Gas coal: 6%; Russian fat coal: 10%;
[0028] 1 / 3 coking coal of G=86: 15%; 1 / 3 coking coal of G=80: 15%;
[0029] G=88 coking coal: 15%; G=81 coking coal: 20%; lean coal: 19%.
[0030] Adjust the ratio of each single coking coal, and control the blended coal to meet the following process parameters: the cohesive index G value is 79-83, the Gibraltar fluidity is 400-2000ddpm, and the Aurya expansion degree b value is <10. Under the condition of no graded crushing, briquette coal technology or tamping coking process, the effective utilization of its resources, among them, the amount of gas coal and lean coal is up to 25%, the amount of coking coal is 35%, and the amount of high-quality coking coal is only 15%. Coal blending cost. The coal blendin...
Embodiment 2
[0032] Russian fat coal is involved in the coking coal blending method, which includes the step of mixing individual coking coals. The raw material components and weight percentages of the single coking coal used are: Russian fat coal: 12%; G=88 1 / 3 Coking coal: 15%;
[0033] 1 / 3 coking coal of G=77: 15%; coking coal of G=89: 18%;
[0034] Coking coal with G=79: 20%; Lean coal: 20%.
[0035] Adjust the ratio of each single coking coal, and control the blended coal to meet the following process parameters: the cohesive index G value is 79-83, the Gibraltar fluidity is 400-2000ddpm, and the Aurya expansion degree b value is <10. Under the condition of no graded crushing, briquette coal process or tamping coking process, the effective utilization of its resources, of which the amount of lean coal is 20%, the amount of coking coal is 38%, and the amount of high-quality coking coal is only 18%, which reduces the cost of coal blending. When the coal blending method of the present ...
Embodiment 3
[0037] Russian fat coal participates in the method of coking coal blending, which includes the steps of mixing individual coking coals. The raw material components and weight percentages of the single coking coals used are:
[0038] Gas coal: 5%; Russian fat coal: 8%;
[0039] 1 / 3 coking coal of G=87: 18%; 1 / 3 coking coal of G=72: 14%;
[0040] Coking coal with G=88: 19%; Coking coal with G=75: 20%; Lean coal: 16%.
[0041] Adjust the ratio of each single coking coal, and control the blended coal to meet the following process parameters: the cohesive index G value is 79-83, the Gibraltar fluidity is 400-2000ddpm, and the Aurya expansion degree b value is <10. Under the condition of no graded crushing, briquette coal process or tamping coking process, the effective utilization of its resources, of which the amount of lean coal is 21%, the amount of coking coal is 39%, and the amount of high-quality coking coal is 19%, reducing the cost of coal blending. The coal blending meth...
PUM
Property | Measurement | Unit |
---|---|---|
cohesion index | aaaaa | aaaaa |
cohesion index | aaaaa | aaaaa |
volatile matter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com