Geopolymer-based glue powder polyphenyl particle thermal insulation mortar
A technology of polystyrene particles and thermal insulation mortar, applied in the field of building materials, can solve the problems of slow drying speed, low surface strength, easy weathering, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Example 1
[0024] Formula one of the present invention:
[0025] Component Formulation (wt%) Dry powdered water glass (m=2.0) 15 Slag 100 mesh 75 secondary fly ash 4.46 polyamide fiber 0.04 wood fiber 0.6 Calcium stearate 0.3 SDBS 0.5 Silica fume 4.1 total 100.00
[0026] Preparation:
[0027] (1) Weigh various raw materials according to the proportion, put them into the gravity-free mixer and stir them evenly.
[0028] (2) When using, add 7.5L of polystyrene particles and 0.52kg of water per kilogram of rubber powder, and mix well before using.
Embodiment 2
[0030] Formula two of the present invention:
[0031] Component Formulation (wt%) Dry powdered water glass (m=2.8) 25 Slag 600 mesh 65 First grade fly ash 4.86 Polypropylene fibers 0.04 wood fiber 0.4 Calcium stearate 0.3 Sodium dodecyl sulfate 0.4 Silica fume 4 total 100.00
[0032] Preparation and construction method:
[0033] (1) Weigh various raw materials according to the proportion, put them into the gravity-free mixer and stir them evenly.
[0034] (2) When using, add 6L of granules and 0.5kg of water per kilogram of rubber powder, and mix well before using.
Embodiment 3
[0036] Formula three of the present invention:
[0037] Component Formulation (wt%) Dry powdered water glass (m=2.2) 20 Slag 400 mesh 68 1. Secondary fly ash mixing 5.05 polyester fiber, polyamide fiber 0.05 wood fiber 0.4 Calcium stearate 0.3 Sodium dodecylbenzene sulfonate and sodium dodecyl sulfate mixture 0.2 Silica fume 6 total 100.00
[0038] Preparation and construction method:
[0039] (1) Weigh various raw materials according to the proportion, put them into the gravity-free mixer and stir them evenly.
[0040] (2) When using, add 8L of granules and 0.6kg of water per kilogram of rubber powder, and mix well before using.
PUM
Property | Measurement | Unit |
---|---|---|
length | aaaaa | aaaaa |
length | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap