Old wood archaizing process
A kind of old wood and craftsmanship technology, applied in the direction of wood processing equipment, manufacturing tools, etc., can solve the problems of complexity, furniture quality, quality and appearance, etc., and achieve the effect of high texture and simple processing method
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2015-05-20
Abstract
Description
technical field
[0001] The invention relates to a method for reprocessing old wood, in particular to an antique craft of old wood, which belongs to the technical field of wood processing. Background technique
[0002] With the improvement of people's living standards, the personalized demand for home decoration is also constantly increasing. Facing the ever-changing product competition in the furniture market, some individual furniture, such as antique furniture, is also coming out of the market. Most of the products produced by the original antique furniture companies are sold abroad to meet the needs of foreign people for Chinese antique furniture. , There is also room for appreciation, so it is also popular in the current home improvement market.
[0003] Generally, common antique furniture can be made by the following methods: (1) Old materials and new works: repair the old furniture, and re-do the repaired parts. Some old furniture is old and difficult to repair. The p...
Examples
Embodiment 1
[0031] Embodiment 1 Adopt the following steps to carry out antique processing of old wooden door panels:
[0032] (1) Saw marks on the white body: use a band saw to make saw marks on the surface of the material;
[0033] (2) White body sanding: Use 150# sandpaper to sand along the wood grain to remove the burrs on the surface;
[0034] (3) Bleaching: After white body sanding, use bleaching water with a concentration of 15% for the first bleaching for 15 minutes. After the first bleaching, prepare sodium hydroxide solution for the second bleaching, bleaching for 5 Minutes; Sodium hydroxide solution preparation: Sodium hydroxide and water are mixed uniformly by the weight ratio of 1:20;
[0035] (4) Drying: Dry the material after twice bleaching at 58°C to a moisture content of 12%;
[0036] (5) Sanding: use 150# sandpaper to sand along the wood grain;
[0037] (6) Sweeping black water: evenly brush the black water prepared according to the ratio on the material; black water ...
Embodiment 2
[0044] Embodiment 2 adopts the following steps to carry out antique processing of old wood planks:
[0045] (1) Saw marks on the white body: use a band saw to make saw marks on the surface of the material;
[0046] (2) White body sanding: Use 150# sandpaper to sand along the wood grain to remove the burrs on the surface;
[0047] (3) Bleaching: After white body sanding, first bleach with 30% bleaching water for 10 minutes, after the first bleaching, prepare sodium hydroxide solution for the second bleaching, and bleach for 3 minutes; Preparation of sodium hydroxide solution: mix sodium hydroxide and water evenly in a weight ratio of 1:18;
[0048] (4) Drying: Dry the material after twice bleaching at 55°C to a moisture content of 11%;
[0049] (5) Sanding: use 150# sandpaper to sand along the wood grain;
[0050](6) Sweeping black water: evenly brush the black water prepared according to the ratio on the material; black water preparation concentration: mix sodium iodate and...
Embodiment 3
[0057] Embodiment 3 Adopt the following steps to carry out antique processing of old wooden door panels:
[0058] (1) Saw marks on the white body: use a band saw to make saw marks on the surface of the material;
[0059] (2) White body sanding: Use 150# sandpaper to sand along the wood grain to remove the burrs on the surface;
[0060] (3) Bleaching: After white body sanding, first bleach with 20% bleaching water for 12 minutes, after the first bleaching, prepare sodium hydroxide solution for the second bleaching, bleaching 4 minute; sodium hydroxide solution preparation: sodium hydroxide and water are mixed uniformly by the weight ratio of 1: 22;
[0061] (4) Drying: Dry the material after twice bleaching at 60°C to a moisture content of 10%;
[0062] (5) Sanding: use 150# sandpaper to sand along the wood grain;
[0063] (6) Sweeping black water: evenly brush the black water prepared according to the ratio on the material; black water preparation concentration: mix sodium ...