Method for Pretreating Softwood Pulp and Hardwood Pulp with Neutral Cellulase
A technology of neutral cellulase and softwood pulp, applied in the field of papermaking, can solve the problems of high energy consumption, achieve the effects of improving product quality, improving paper strength, and reducing refining power
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] The method for neutral cellulase pretreatment softwood pulp and hardwood pulp, comprises the following steps:
[0027] (1) Add 1 / 3 volume of pulping water into the medium-consistency hydraulic pulper tank. The pH value of the pulping water is 6.5-7.0, and the water temperature is 40-45°C. When the water temperature is lower than 40°C, use a drying Cylinder exhaust steam heats pulping water;
[0028] (2) Start the medium-consistency hydraulic pulper, add thermophilic Chaetomium cellulase for papermaking beating to the medium-consistency hydraulic pulper, and the dosage is 0.2kg of thermophilic wool for papermaking pulping per ton of pulp. For shell fungus cellulase, put the coniferous pulp and broad-leaved pulp into the medium-concentration hydraulic pulper at a ratio of 12:88, and keep the thermophilic Chaetomium cellulase and pulp in the medium-concentration hydraulic pulper for papermaking pulping. The reaction time in the pulper is 30 minutes;
[0029] (3) The pret...
Embodiment 2
[0032] The method for neutral cellulase pretreatment softwood pulp and hardwood pulp, comprises the following steps:
[0033] (1) Add 1 / 3 volume of pulping water into the medium-consistency hydraulic pulper tank. The pH value of the pulping water is 6.5-7.0, and the water temperature is 40-45°C. When the water temperature is lower than 40°C, use a drying Cylinder exhaust steam heats pulping water;
[0034] (2) Start the medium-consistency hydraulic pulper, add thermophilic Chaetomium cellulase for papermaking beating to the medium-consistency hydraulic pulper, and the dosage is 0.1kg of thermophilic wool for papermaking beating per ton of pulp. For shell fungus cellulase, put the coniferous pulp and broad-leaved pulp into the medium-concentration hydraulic pulper at a ratio of 12:88, and keep the thermophilic Chaetomium cellulase and the pulp in the medium-concentration hydraulic pulper for pulping. The reaction time in the pulper is 35 minutes;
[0035] (3) The pretreated s...
Embodiment 3
[0038] The method for neutral cellulase pretreatment softwood pulp and hardwood pulp, comprises the following steps:
[0039] (1) Add 1 / 3 volume of pulping water into the tank body of the low-consistency hydraulic pulper. The pH value of the pulping water is 6.5-7.0, and the water temperature is 40-45°C. When the water temperature is lower than 40°C, use an oven Cylinder exhaust steam heats pulping water;
[0040] (2) Start the low-consistency hydraulic pulper, add thermophilic Chaetomium cellulase for papermaking beating into the low-consistency hydraulic pulper, and the dosage is 0.3kg of thermophilic wool for papermaking pulping per ton of pulp. For shell fungus cellulase, put the coniferous pulp and broad-leaved pulp into the medium-consistency hydraulic pulper at a ratio of 12:88, and keep the thermophilic Chaetomium cellulase and the pulp used for pulping in low-concentration hydraulic pulverization. The reaction time in the pulper is 35 minutes;
[0041] (3) The pretr...