Looking for breakthrough ideas for innovation challenges? Try Patsnap Eureka!

Flotation process of mixed type collophosite containing organic carbonaceous silicon calcium

A mixed-type collophosite technology, applied in flotation, solid separation, etc., can solve the problems of increasing the amount of collector, increasing the cost of mineral processing, and reducing the content, so as to avoid mechanical inclusion and transportation difficulties, reduce the cost of mineral processing, The effect of reducing the amount of foam

Inactive Publication Date: 2017-02-15
WUHAN INSTITUTE OF TECHNOLOGY
View PDF4 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Especially in the beneficiation of low-grade silicon-calcium mixed type collophosite containing a small amount of organic carbon, conventional direct flotation and single reverse flotation can only reduce the content of one of the gangue minerals, and cannot obtain better quality Phosphate concentrate
At present, the more reasonable separation and enrichment process of this type of phosphate rock is positive and negative flotation. This process uses anionic collectors to remove carbonate minerals and silicate minerals in different acid-base pulps. , to obtain high-grade phosphate concentrate, but in the forward and reverse flotation of silicon-calcium mixed phosphate rock containing organic carbon, due to the presence of organic carbon, a large amount of anionic collectors will be adsorbed, and the collection will be doubled. The amount of agent used, otherwise, the flotation cannot be completed
Increasing the amount of collector will increase the amount of foam in positive flotation, reduce the selectivity of flotation, easily cause mechanical inclusion of foam and difficulty in transportation, make the flotation process difficult to control and stabilize, and lead to a substantial increase in beneficiation costs
Because of the above-mentioned technical and economic problems, the industrialization of the flotation process of organic carbon silicon-calcium mixed collophosite is restricted.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0030] Ore raw materials: using organic carbon silicon-calcium mixed type collophosite. The main chemical composition is: P 2 o 5 The mass percentage content is 20.34%, the mass percentage content of MgO is 3.56%, and the SiO 2 The mass percentage of organic carbon is 16.57%, and the mass percentage of organic carbon is 2.45%.

[0031] The organic carbon silicon calcium mixed type collophosite is crushed and ground with water to obtain a pulp with a mass concentration of 20%, and an anionic fatty acid collector and a foaming agent diethyl phthalate are added to the pulp to mix, and the pulp is mixed by stirring And use the flotation machine to carry out flotation decarbonization roughing, the resulting foam product is carbon-containing tailings, and the product in the tank enters the positive flotation desiliconization process; the ratio of the amount of anionic fatty acid collector to the original ore is 2.0 kg / t, the ratio of the amount of foaming agent added to the raw or...

Embodiment 2

[0037] Ore raw materials: using organic carbon silicon-calcium mixed type collophosite. The main chemical composition is: P 2 o 5 The mass percentage content is 24.12%, the mass percentage content of MgO is 4.45%, and the SiO 2 The mass percentage of organic carbon is 15.46%, and the mass percentage of organic carbon is 3.67%.

[0038] The organic carbon silicon-calcium mixed type collophosite is crushed and ground with water to obtain a pulp with a mass concentration of 40%, and an anionic fatty acid collector and a foaming agent diethyl phthalate are added to the pulp to mix, and the pulp is mixed with stirring And use the flotation machine to carry out flotation decarbonization roughing, and the products in the obtained tank enter the positive flotation desiliconization process; the ratio of the addition amount of the anionic fatty acid collector to the raw ore is 1.4kg / t, and the foaming agent The ratio of added amount to raw ore is 0.3kg / t. The resulting foam product i...

Embodiment 3

[0049] Ore raw materials: using organic carbon silicon-calcium mixed type collophosite. The main chemical composition is: P 2 o 5 The mass percentage content is 22.45%, the mass percentage content of MgO is 5.46%, and the SiO 2 The mass percentage of organic carbon is 16.94%, and the mass percentage of organic carbon is 2.67%.

[0050] The organic carbon silicon-calcium mixed type collophosite is crushed and ground with water to obtain a pulp with a mass concentration of 25%, and an anionic fatty acid collector and a foaming agent diethyl phthalate are added to the pulp to mix, and the pulp is adjusted by stirring And use the flotation machine to carry out flotation decarbonization roughing, the resulting foam product is carbon-containing tailings, and the product in the tank enters the positive flotation desiliconization process; the ratio of the amount of anionic fatty acid collector to the original ore is 1.5 kg / t, the ratio of the amount of foaming agent added to the raw...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a flotation decarburization and direct and reverse flotation process for silicon-calcium mixed collophanite containing organic carbon. The mass percentage of the organic carbon in the silicon-calcium mixed collophanite ranges from 1% to 10%. The flotation process includes sequentially performing flotation decarburization, direct flotation desiliconization and reverse flotation magnesium removal. A flotation decarburization technology includes adding water into the silicon-calcium mixed collophanite containing the organic carbon and crushing and grinding the silicon-calcium mixed collophanite containing the organic carbon to obtain ore pulp with the mass concentration ranging from 20% to 40%; adding collecting agents and foaming agents into the ore pulp and mixing the ore pulp, the collecting agents and the foaming agents with one another; stirring and regulating the pulp and performing flotation on the ore pulp by the aid of a flotation machine to obtain foam products which are tailings containing carbon; implementing a direct flotation desiliconization technology on products in tanks; then sequentially implementing direct and reverse flotation on the products. The flotation decarburization and direct and reverse flotation process has the advantages that organic carbon gangue can be eliminated by means of flotation implemented by the aid of the anionic fatty acid collecting agents and the diethyl phthalate foaming agents, accordingly the content of the organic carbon in the ore pulp can be reduced, consumption of the collecting agents can be decreased, the high quantity of direct flotation foam can be reduced, and the flotation selectivity can be improved.

Description

technical field [0001] The invention belongs to the technical field of phosphate ore beneficiation, and in particular relates to an organic carbon silicon-calcium mixed type collophosite flotation decarbonization-direct and reverse flotation process. Background technique [0002] Phosphate rock is an essential basic raw material for the production of phosphate fertilizers and phosphorus chemical products. my country's phosphate resource reserves are 16.786 billion tons, with an average grade of 16.95%. The high-grade ore that can be directly used can only be mined for more than ten years. Poor dissociation and high content of gangue minerals such as silicate minerals and carbonate minerals. For this type of ore, it is necessary to exclude gangue minerals such as silicate minerals and carbonate minerals in the beneficiation process to meet the requirements. Phosphorus chemical industry requirements, its development and utilization is a worldwide problem. Especially for the be...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): B03D1/00
Inventor 罗惠华李亮汤家焰饶欢欢杨婕陈慧
Owner WUHAN INSTITUTE OF TECHNOLOGY
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products