Method for manufacturing viscose fiber/wool/polyester fiber blended fabric
A polyester fiber and viscose fiber technology, applied in the textile field, can solve the problems of easy falling of cotton net, poor weaving, easy clogging of bell mouth, etc. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] In the preparation method of a kind of viscose fiber / wool / polyester fiber blended fabric provided in this embodiment, the selected warp and weft thread materials are calculated in parts by mass: 25 parts of wool, 14 parts of polyester fiber, 6 parts of mulberry silk, viscose 58 parts of rubber fiber, 33 parts of combed cotton, 16 parts of superfine polyester, 92 / 2 warp and 48 / 1 weft;
[0025] The preparation process of blended fabrics is cotton cleaning→carding→strip mixing→head needle→two needles→three needles→four needles→roving→spun yarn→weaving operation, in which: the weaving process also includes warping→doubling→folding Twisting→vacuum setting→sizing and air jet operation;
[0026] Mixing→head needle→second needle→three needle→four needle→roving→spinning operation, control relative humidity 70%-75%, temperature 26-30℃;
[0027] In the carding process: the speed ratio of kunlin and licker-in rollers for viscose fiber is 2.5:3, the gauge of the cylinder cover is 0...
Embodiment 2
[0034] In the preparation method of a kind of viscose fiber / wool / polyester fiber blended fabric provided in this embodiment, the selected warp and weft thread materials are calculated in parts by mass: 45 parts of wool, 11 parts of polyester fiber, 5 parts of mulberry silk, viscose 56 parts of rubber fiber, 25 parts of combed cotton, 16 parts of superfine polyester, 92 / 2 warp and 48 / 1 weft;
[0035] The preparation process of blended fabrics is cotton cleaning→carding→strip mixing→head needle→two needles→three needles→four needles→roving→spun yarn→weaving operation, in which: the weaving process also includes warping→doubling→folding Twisting→vacuum setting→sizing and air jet operation;
[0036] Mixing→head needle→second needle→three needle→four needle→roving→spinning operation, control relative humidity 70%-75%, temperature 26-30℃;
[0037] In the carding process: the speed ratio of kunlin and licker-in rollers for viscose fiber is 2.5:3, the gauge of the cylinder cover is 0...
PUM
| Property | Measurement | Unit |
|---|---|---|
| Winding density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More