IoT new transport bag for packaging raw ecological food and method of use thereof
A technology of the Internet of Things and transport bags, applied in the field of the Internet of Things, can solve the problems of uncontrollable management of the transportation process, reduction of user trust, and user inability to identify, etc., to achieve rapid promotion and use, ensure no change, and enhance competitiveness.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment a
[0037] Nanoscale aluminum oxide 1.8%, polylactic acid / propylene carbonate blend 4.3%, stearic acid coupling agent 2.1%, paraffin 6.2%, and the balance is a degradable polymer; wherein the degradable polymer The molecular formula is:
[0038]
[0039] In the formula, m is 15-25, and n is 10-20. The nano-scale alumina is 6000-8000 mesh. The weight average molecular weight of the polylactic acid / propylene carbonate blend is 50,000-80,000. The thickness of the bag body is 0.04mm.
[0040] The tensile strength is 45.3MPa, the elongation is 445.3%, and the 6-week degradation rate is 92%.
Embodiment b
[0042] Nanoscale aluminum oxide 1.5%, polylactic acid / propylene carbonate blend 2.2%, stearic acid coupling agent 3.2%, paraffin 5.2%, and the balance is degradable polymer; wherein the degradable polymer The molecular formula is:
[0043]
[0044] In the formula, m is 15-25, and n is 10-20. The nano-scale alumina is 6000-8000 mesh. The weight average molecular weight of the polylactic acid / propylene carbonate blend is 50,000-80,000. The thickness of the bag body is 0.04mm.
[0045] The tensile strength is 48.5MPa, the elongation is 346.2%, and the degradation rate is 88% in 6 weeks.
Embodiment c
[0047] Nanoscale aluminum oxide 3.5%, polylactic acid / propylene carbonate blend 3.5%, stearic acid coupling agent 1.8%, paraffin 5.5%, and the balance is a degradable polymer; wherein the degradable polymer The molecular formula is:
[0048]
[0049] In the formula, m is 15-25, and n is 10-20. The nano-scale alumina is 6000-8000 mesh. The weight average molecular weight of the polylactic acid / propylene carbonate blend is 50,000-80,000. The thickness of the bag body is 0.04mm.
[0050] The tensile strength is 52.1MPa, the elongation is 384.3%, and the degradation rate is 93% in 6 weeks.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com