Vortex spinning knitted fabric with stranded yarn effects
A technology for vortex spinning and knitting fabrics, applied in the field of textile manufacturing, can solve the problems of difficult to ensure uniform yarn quality, the need to improve the wearability of fabrics, and difficult to control the weaving process, so as to achieve good anti-pilling characteristics, good moisture absorption and ventilation , the effect of soft feel
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] The weave is single jersey. Horizontal density: 44.5 longitudinal rows / 10cm; longitudinal density: 60 rows / 10cm.
[0019] Needle size: 12G, knitted on a computerized flat knitting machine.
[0020] Yarn: 16S single-ply viscose yarn is used.
[0021] Gram weight: 288 grams / square meter.
[0022] Product process:
[0023] Air-jet vortex spinning→rewinding→woven piece→sleeving→flat car→hand sewing→washing→drying→ironing→packing→warehousing.
[0024] Before air-jet vortex spinning, the viscose yarn is pre-humidified to make the moisture content of the yarn reach 15%.
[0025] In the process of air-jet vortex spinning, the drawing speed is 230m / min, the spinning air pressure is 0.63Mpa, the length of the threading needle is 1.7mm, the diameter of the nozzle hole is 0.53mm, and the feeding ratio is 0.90.
[0026] Authoritative testing by the National Textile Product Quality Supervision and Inspection Center (Jiangyin): According to GB18401-2010 "National Basic Safety Tec...
Embodiment 2
[0029] The weave is single jersey. Horizontal density: 44.5 longitudinal rows / 10cm; longitudinal density: 60 rows / 10cm.
[0030] Needle size: 12G, knitted on a computerized flat knitting machine.
[0031] Yarn: 16S single-ply viscose yarn is used.
[0032] Gram weight: 288 grams / square meter.
[0033] Product process:
[0034] Air-jet vortex spinning→rewinding→woven piece→sleeving→flat car→hand sewing→washing→drying→ironing→packing→warehousing.
[0035] Before air-jet vortex spinning, the viscose yarn is pre-humidified to make the moisture content of the yarn reach 14%.
[0036] During the air-jet vortex spinning process, the drawing speed is 230m / min, the spinning air pressure is 0.63Mpa, the lead needle length is 1.7mm, the nozzle hole diameter is 0.53mm, and the feed ratio is 0.89.
[0037] Color fastness to washing: grade 4-5 (technical requirement 3); color fastness to water: grade 4-5 (technical requirement 3); color fastness to acid and sweat: grade 4-5 (technical ...
Embodiment 3
[0039] The weave is single jersey. Horizontal density: 44.5 longitudinal rows / 10cm; longitudinal density: 60 rows / 10cm.
[0040] Needle size: 12G, knitted on a computerized flat knitting machine.
[0041] Yarn: 16S single-ply viscose yarn is used.
[0042] Gram weight: 288 grams / square meter.
[0043] Product process:
[0044] Air-jet vortex spinning→rewinding→woven piece→sleeving→flat car→hand sewing→washing→drying→ironing→packing→warehousing.
[0045] Before air-jet vortex spinning, the viscose yarn is pre-humidified to make the moisture content of the yarn reach 13%.
[0046] In the process of air-jet vortex spinning, the yarn drawing speed is 230m / min, the spinning air pressure is 0.63Mpa, the length of the threading needle is 1.7mm, the nozzle hole diameter is 0.53mm, and the feeding ratio is 0.92.
[0047] Color fastness to washing: grade 4-5 (technical requirement 3); color fastness to water: grade 4-5 (technical requirement 3); color fastness to acid and sweat: gr...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com