Looking for breakthrough ideas for innovation challenges? Try Patsnap Eureka!

One-component polyurea coating and preparation method thereof

A coating and polyurea technology, applied in the field of one-component polyurea coating and its preparation, can solve the problems of low coating hardness, tensile strength and elongation, difficult industrialization, poor bonding force between coating and substrate, etc.

Active Publication Date: 2018-03-13
刘朝辉
View PDF3 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Due to the fast reaction speed and very short time, it also brings problems to the normal use of the coating. The film-forming substance is too fast, which will produce some fatal surface defects, which makes the bonding force between the coating and the substrate relatively poor. There may even be discontinuous coatings; at the same time, there are problems such as poor protective effect of polyurea coatings and low tensile strength
The solid content of the one-component polyurea type polyurethane coating that is currently used in this field is generally below 70%, and the coating hardness, tensile strength and elongation are low relative to the two-component coating, especially in some specific occasions (such as Acetone, ethylene glycol, environments with high oil content or environments above 100°C), lower tensile strength and elongation, and are greatly restricted during use
The single-component polyurea polyurethane coating disclosed in Chinese patent CN102101967A is made of blocked isocyanate and blocked polyetheramine. Although the tensile strength and elongation of the coating are improved to a certain extent, the method is complicated. It consumes raw materials and energy, and it is difficult to realize industrialization. At the same time, the one-component polyurea made of end-capped polyetheramine and isocyanate prepolymer has poor storage stability, and is not suitable for environments with high engine oil content.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • One-component polyurea coating and preparation method thereof
  • One-component polyurea coating and preparation method thereof
  • One-component polyurea coating and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0028] Add 50ml of amino-terminated polyether (product of Yangzhou Chenhua Technology Group Co., Ltd., number-average molecular weight is 2000) in a four-necked flask with agitator, thermometer, dropping funnel, and reflux condenser, then use the dropping funnel to drop Add 55-57ml of cyclobutanone (product of Shanghai Lingfeng Chemical Reagent Co., Ltd., chemically pure), and then add 15ml of polyamine (diethylenetriamine, product of Shanghai Lingfeng Chemical Reagent Co., Ltd., chemically pure) solution to promote chain extension The reaction proceeds. While adding the solution dropwise, stir with a glass rod, heat in a water bath to control the reaction temperature at 80°C, and control the dropping rate below 2ml / min. After the dropwise addition is completed, keep warm and reflux for 30 minutes. When the solution gradually turns into a light yellow liquid accompanied by the generation of ammonia-like gas, it indicates that ketimine is formed and the terminal amino group has...

Embodiment 2

[0031] Polyurea coating performance test method

[0032] (1) Tensile test

[0033] Laboratory equipment

[0034]Tensile testing machine: Jiangsu Mingzhu Experimental Machinery Co., Ltd. MZ-4000D electronic universal testing machine, the displacement measurement accuracy is within ±0.5% of the indicated value, the deformation measurement accuracy is within ±0.5% of the indicated value, and the effective stretching distance is 900mm. The stretching speed is 6mm / min-500mm / min. Slicer: cut the type I dumbbells that meet the requirements of GB / T 528-1998 test pieces. Thickness gauge: pressure (100 ± 10) g, measuring surface diameter (10 ± 1) mm, minimum graduation 0.01 mm. Vernier caliper: accuracy ± 0.02mm.

[0035] experimental method

[0036] Cut 6 dumbbell-shaped specimens, place the specimens under standard conditions for at least 2 hours, then draw two parallel marking lines with a distance of 65mm on the specimens with a ruler, and measure the middle and both ends of th...

Embodiment 3

[0066] The polyurea coating performance test result that embodiment 1 makes

[0067] (1) Experimental results of physical performance test of single-component polyurea coating material

[0068] The performance of the one-component polyurea sample prepared by cyclobutanone modification and the conventional two-component polyurea sample is compared, and the results are shown in Table 1.

[0069] Table 1 Comparison of relative properties between one-component polyurea of ​​the present invention and two-component polyurea samples

[0070] project

Two-component polyurea

One-component polyurea of ​​the present invention

Solid content

83

85.2

Surface dry time / h

5~6

2~3

Working time / h

18~20

10~12

Gel time / s

5

19

Coating adhesion / MPa

7

21

Tensile strength / MPa

12.5

25.1

Elongation at break / %

250

429

100% modulus stress / MPa

3.3

1.8

300% modulus stress / MPa

6....

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
gel timeaaaaaaaaaa
adhesivityaaaaaaaaaa
tensile strengthaaaaaaaaaa
Login to View More

Abstract

The invention discloses a single-component polyurea coating. Cyclobutanone is used as a cosolvent and a closing agent at the same time; terminating amino of amino-terminated polyoxypropylene ether is subjected to chemical closing; an intermediate (ketoimine) obtained after closure and a component containing -NCO cannot generate a chemical reaction in a condition of air (moisture) isolation, and can coexist in the same system; the mixture of the intermediate (ketoimine) is subjected to closure relief under the action of moisture once being in contact with air; the terminating amino is released; amino-NH2 quickly generates a reaction with the -NCO, so as to form a urea bond. The single-component polyurea coating has excellent physicochemical properties of higher mechanical properties, wear resistance, wet skid prevention, corrosion prevention and the like, is less influenced by solvents (acetone, ethylene glycol and the like), and can adapt to an environment of which the content of an organic solvent is high or the concentration of engine oil is higher. The single-component polyurea coating provided by the invention has the advantage that a preparation method is simple, and is suitable for industrialized production.

Description

technical field [0001] The invention relates to a polyurea coating, in particular to a single-component polyurea coating and a preparation method thereof. Background technique [0002] Buildings exposed to sulfate, chloride, CO 2 Under the action of corrosive media in the air such as gas, it will cause rust and corrosion of steel bars, and cracks will occur when concrete absorbs water and expands, thereby reducing the service life of buildings. Spray Polyurea Elastomer technology (SPUA technology for short) is a kind of thick coating construction technology that can be rapidly formed on the surface of objects. layer, and has good wear resistance and impact resistance and marine weather aging resistance, which can better reduce the corrosion rate of buildings under the influence of severe weather. Polyurea elastomer is composed of terminal isocyanate prepolymer (—NCO) and amino compound (—NH 2 ) The high-molecular polymer with urea bonds generated by the reaction of the cu...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C09D175/02C09D5/08C08G18/32C08G18/50C08G18/66
CPCC08G18/3228C08G18/3246C08G18/5024C08G18/6685C09D5/08C09D5/18C09D175/02
Inventor 刘朝辉杨宏波刘娜王飞贾艺凡叶圣天班国东丁逸栋林锐陶睿
Owner 刘朝辉
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products