Embodiment 1
[0036] In this embodiment, the active snow-melting material for asphalt pavement is prepared as follows:
[0037] The material is mainly composed of deicing agent, diluent, adhesive and curing agent, wherein the parts by weight of each component are: anhydrous calcium chloride 53; sodium lauryl sulfate crystal 9; phthalic anhydride 10; Liquid epoxy resin (E-51) 28.
[0038] The preparation method of the active snow-melting material for highway pavement comprises the following steps:
[0039] 1) According to the mass fraction of the components, select anhydrous calcium chloride, sodium lauryl sulfate crystals and phthalic anhydride to mix and powder, and set aside;
[0040] 2) Under certain conditions, the mixed solid powder obtained in step 1) and epoxy resin (E-51) are mixed evenly by mechanical stirring to obtain a paste;
[0041] 3) Granulate the paste obtained in step 2) to obtain 0.1-5 mm particles;
[0042] 4) Dry and solidify the particles obtained in step 3) at 70-9...
Embodiment 2
[0044] In this embodiment, the active snow-melting material for asphalt pavement is prepared as follows:
[0045] The material is mainly composed of deicing agent, diluent, adhesive and curing agent, wherein the parts by weight of each component are: anhydrous calcium chloride 50, sodium chloride 15, sodium lauryl sulfate crystal 6; liquid Acetic anhydride 15; liquid epoxy resin (MF5110) 14.
[0046] The preparation method of the asphalt pavement active snow-melting material comprises the following steps:
[0047] 1) According to the mass fraction of the components, select anhydrous calcium chloride, sodium chloride, and sodium lauryl sulfate crystals to mix and powder, and set aside;
[0048] 2) Under certain conditions, the mixed solid powder obtained in step 1), acetic anhydride, and epoxy resin (MF5110) are mixed uniformly by mechanical stirring to obtain a paste;
[0049] 3) The paste obtained in step 2) is granulated to obtain 0.1~5mm particles;
[0050]4) Dry and sol...
Embodiment 3
[0052] In this embodiment, the active snow-melting material for asphalt pavement is prepared as follows:
[0053] The material is mainly composed of deicing agent, diluent, adhesive and curing agent, wherein the parts by weight of each component are: anhydrous calcium chloride 53; hydroxy ketone, 9 parts, hydroxy ketone is composed of formaldehyde, acetone and sodium sulfite Synthesized under conditions; 10 parts of phthalic anhydride; 28 parts of liquid epoxy resin (E-51).
[0054] The preparation method of the asphalt pavement active snow-melting material comprises the following steps:
[0055] 1) According to the mass fraction of the components, select anhydrous calcium chloride, hydroxyketone and phthalic anhydride to mix and powder, and set aside;
[0056] 2) Under certain conditions, the solid powder obtained in step 1) and the liquid epoxy resin (E-51) are mixed evenly by mechanical stirring to obtain a paste;
[0057] 3) The paste obtained in step 2) is granulated to...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com