Embodiment 1
[0040] Each of the following material components is measured in parts by mass.
[0041] (1) Toner dispersion: completed in two steps. Add 30 parts of water and 50 parts of Clariant blue toner (C.I.15: 3 blue) into the grinder, and use a nano grinder (Pengyi WBS-12, on the website of Qinhuangdao Pengyi Chemical Machinery Co., Ltd., the same below) to grind 30 minutes. Then add 10 parts of color paste dispersant polycarboxylate polymer macromolecule dispersant Demol P, grind for 30 minutes, then slowly add remaining 50 parts of toner and 70 parts of water, grind and disperse until grinding color paste particle size D50 200-500 nanometers (measured by a laser particle size analyzer, the maximum particle size does not exceed 500nm).
[0042] (2) Color paste preparation: Add 50 parts of self-crosslinking polyurethane resin (TakeLacWS-6021) and 10 parts of wetting agent (glycerin) to the dispersed toner in step (1), mix for 10 minutes, and adjust the color paste with water The so...
Embodiment 2
[0047] Each of the following material components is measured in parts by mass.
[0048] (1) Toner dispersion: completed in two steps. Add 30 parts of water and 30 parts of BASF blue toner (C.I. 60 blue) into the grinder, and use the nano grinder to grind for 30 minutes. Then add 20 parts of color paste dispersant polycarboxylate polymer macromolecule dispersant Demol P, after grinding for 30 minutes, slowly add remaining 70 parts of toner and 100 parts of water, grind and disperse until grinding color paste particle size D50 200-500 nanometers.
[0049] (2) Color paste preparation: Add 100 parts of self-crosslinking polyurethane resin (TakeLac WS-6021) and 10 parts of wetting agent (glycerin) to the dispersed toner in step (1), mix for 10 minutes, and adjust the color with water The solids content in the pulp consistency was 40%.
[0050] (3) Color fixation for papermaking: before the color paper is formed, add color paste with 2Kg of 1 ton of pulp and 40% solid content in ...
Embodiment 3
[0054] Each of the following material components is measured in parts by mass.
[0055] (1) Toner dispersion: completed in two steps. Add 30 parts of water and 60 parts of Clariant blue toner (C.I.15:3 blue) into the grinder, and grind for 30 minutes with a nano grinder. Then add 30 parts of color paste dispersant polycarboxylate polymer macromolecule dispersant Demol P, after grinding for 30 minutes, slowly add remaining 40 parts of toner and 120 parts of water, grind and disperse until grinding color paste particle size D50 200-500 nanometers.
[0056] (2) Color paste preparation: Add 120 parts of self-crosslinking polyurethane resin (TakeLac WS-6021) and 20 parts of wetting agent (glycerin) to the dispersed toner in step (1), mix for 10 minutes, and adjust the color with water The solids content in the pulp consistency was 35%.
[0057] (3) Color fixation for papermaking: before the color paper is formed, add color paste with 2Kg of 1 ton of pulp and 35% solid content in...