A technology for hydrorefining and catalyst, applied in molecular sieve catalysts, chemical instruments and methods, organic compounds/hydrides/coordination complex catalysts, etc., can solve the problems of waste of metal salts, easy precipitation, and low stability of impregnation solution. , to achieve the effect of improving the hydrodesulfurization activity and reducing the cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0046] Take 50g of pseudo-boehmite and 30g of TS-1 molecular sieve, and mix them evenly. Add 4g of scallop powder, mix well, dropwise add an aqueous solution containing 4g of nitric acid and 4g of citric acid and knead, extrude into a clover shape of 1.5mm, freeze-dry, and then roast at 550°C for 4h to make a carrier. Use Ni again 6 [WNi 3 (H 2 O) 2 (ZnW 9 o 34 ) 2 ] The impregnated solution was impregnated with equal volume, freeze-dried, and calcined at 400°C for 4h to obtain catalyst A.
Embodiment 2
[0048] Take 70g of pseudo-boehmite and 20g of TS-1 molecular sieve, and mix them evenly. Add 4g of scallop powder, mix well, dropwise add an aqueous solution containing 4g of nitric acid and 4g of citric acid and knead, extrude into a clover shape of 1.5mm, freeze-dry, and then roast at 550°C for 4h to make a carrier. Use Ni again 6 [WNi 3 (H 2 O) 2 (ZnW 9 o 34 ) 2 ] The impregnated solution was impregnated with an equal volume, freeze-dried, and calcined at 400°C for 4h to obtain Catalyst B.
Embodiment 3
[0050] Take 50g of pseudo-boehmite and 35g of TS-1 molecular sieve, and mix them evenly. Add 4g of scallop powder, mix well, dropwise add an aqueous solution containing 4g of nitric acid and 4g of citric acid and knead, extrude into a clover shape of 1.5mm, freeze-dry, and then roast at 550°C for 4h to make a carrier. Use Ni again 6 [WNi 3 (H 2 O) 2 (ZnW 9 o 34 ) 2 ] impregnated with equal volumes of the prepared impregnating solution, freeze-dried, and calcined at 400°C for 4 hours to obtain catalyst C.
PUM
| Property | Measurement | Unit |
|---|---|---|
| specific surface area | aaaaa | aaaaa |
| diameter | aaaaa | aaaaa |
| diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 