A chain bead-like particle self-assembled in 2 o 3 Synthetic method of hollow cage and product therefrom
A self-assembly, in2o3 technology, applied in gallium/indium/thallium compounds, chemical instruments and methods, nanotechnology for materials and surface science, etc., to achieve good dispersion, easy operation of equipment, and good repeatability.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] 1.1 32 mL of DMF, 0.4 mL of water, 3.2 mL of acetoin, and 3.2 mL of dimethyl sulfoxide were prepared as a mixed solvent in a beaker, and then 0.3120 g of indium nitrate hydrate (InN 3 O 9 . xH 2 O) and 0.120 g terephthalic acid (C 8 H 6 O 4 ) and 0.0156 g of imidazole (C 3 H 4 N 2 ) was added to the above mixed solvent and stirred for 0.5 h;
[0026] 1.2 Transfer the above solution to the reaction kettle and seal it at 120 °C for 0.5 h;
[0027] 1.3 After the product was centrifuged and washed, it was placed in a muffle furnace, and the temperature was increased from room temperature to 550 °C at a heating rate of 1 °C / min in an air atmosphere, and the product was kept for 2 h.
[0028] The phase structure of the product is as figure 1 As shown, all diffraction peaks are related to In 2 O 3 The standard XRD card (06-0461) remains the same. The microscopic appearance of the product is as figure 2 As shown, the product obtained by the present invention is t...
Embodiment 2
[0030] 2.1 Prepare a mixed solvent of 32 mL of DMF, 0.32 mL of water, 1.6 mL of acetoin, and 1.9 mL of dimethyl sulfoxide in a beaker, and then mix 0.3120 g of InN 3 O 9 . xH 2 O and 0.063 g C 8 H 6 O 4 and 0.0110 g of C 3 H 4 N 2 was added to the above mixed solvent and stirred for 0.5 h;
[0031]2.2 Transfer the above solution to the reaction kettle and seal it at 100 °C for 0.2 h;
[0032] 2.3 After the product was centrifuged and washed, it was placed in a muffle furnace, and the temperature was increased from room temperature to 450 °C at a heating rate of 1 °C / min in an air atmosphere, and the product was kept for 1 h.
[0033] In 2 O 3 The nano-hollow cage has a relatively uniform size and good dispersibility, with a size of 130-150 nm, and the structural unit is a chain bead-like particle with a particle size of about 14-18 nm.
Embodiment 3
[0035] 3.1 Prepare a mixed solvent of 32 mL of DMF, 0.4 mL of water, 2.3 mL of acetoin, and 3.2 mL of dimethyl sulfoxide in a beaker, and then mix 0.312 g of InN 3 O 9 . xH 2 O and 0.095 g C 8 H 6 O 4 and 0.0156 g of C 3 H 4 N 2 was added to the above mixed solvent and stirred for 0.5 h;
[0036] 3.2 Transfer the above solution to the reaction kettle and seal it for 1 h at 130 °C;
[0037] 3.3 After the product was centrifuged and washed, it was placed in a muffle furnace, and the temperature was increased from room temperature to 500 °C at a heating rate of 2 °C / min in an air atmosphere, and kept for 3 h. The product was obtained after the sample was cooled in the furnace.
[0038] In 2 O 3 The nano-hollow cage has a relatively uniform size and good dispersibility, with a size of 560-610 nm, and the structural unit is a chain bead-like particle with a particle size of about 50-59 nm.
PUM
| Property | Measurement | Unit |
|---|---|---|
| size | aaaaa | aaaaa |
| size | aaaaa | aaaaa |
| size | aaaaa | aaaaa |
Abstract