An elastic graphite strong adsorption plugging agent and oil-based drilling fluid
A technology of oil-based drilling fluid and elastic graphite, which is applied in the field of oil-based drilling fluid, can solve problems such as wellbore instability, and achieve the effects of enhanced plugging performance, reduced fluid loss rate, and good compatibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] Weigh 2.5g of elastic graphite powder ground to 200nm, add 65ml of concentrated sulfuric acid, stir and react in an ice bath at -2°C for 30min, then add 2g of sodium nitrate and continue stirring for 30min; slowly add 8g of potassium permanganate, and control the temperature at 20 ℃, stir for 2 hours; raise the temperature to 35℃, let stand for 2 hours, add 150mL of deionized water dropwise, then raise the temperature to 98℃, after a golden yellow suspension appears, add 20mL of hydrogen peroxide, and then add 150mL of deionized Water, ultrasonically dispersed for 1 h; after the reaction, put it into a centrifuge, centrifuge at 5000 rpm for 5 min, then filter, then wash the solid matter with deionized water and absolute ethanol for 3 times, and finally, vacuum dry the solid at 60°C for 24 h to obtain Oxidized elastic graphite.
[0023] Disperse 0.5g of oxidized elastic graphite in 100mL of distilled water, and use ultrasonic treatment for 1h to obtain a uniform solution...
Embodiment 2
[0027]Weigh 3g of elastic graphite powder ground to 200nm, add 80ml of concentrated sulfuric acid, stir and react in an ice bath at -2°C for 35min, then add 2.5g of sodium nitrate and continue stirring for 30min; slowly add 10g of potassium permanganate, and control the temperature to 20 ℃, stirred for 2.0h; raised the temperature to 35℃, stood for 2.5h; added 150mL of deionized water dropwise, then raised the temperature to 98℃, and after a golden yellow suspension appeared, added 20mL of hydrogen peroxide, and then added 150mL of Deionized water, ultrasonic dispersion for 1h; after the reaction, put it in a centrifuge, centrifuge at 5000rpm for 5min, then filter, then wash the solid matter with deionized water and absolute ethanol for 3 times, and finally, vacuum dry the solid at 60°C for 24h , to obtain oxidized elastic graphite.
[0028] Disperse 0.8g of oxidized elastic graphite in 100mL of distilled water, and use ultrasonic treatment for 1 hour to obtain a uniform solut...
PUM
| Property | Measurement | Unit |
|---|---|---|
| density | aaaaa | aaaaa |
| density | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 