[0020] Embodiment 1, take by weighing 7.62 kilograms of ethylene glycol, put in the container, and this container is fixed on the stirrer. Set the speed of the mixer at 400 revolutions per minute.
[0021] Sprinkle 0.85 kg of polyethylene oxide powder weighed in advance into the stirring ethylene glycol at a constant speed with a spoon. The speed of adding is controlled at 0.17 kilograms per minute, promptly with the time of 5 minutes, above-mentioned polyoxyethylene powder is added in the container. Stop the mixer, check whether there is agglomerate in the material, if there is, continue to stir; if there is no agglomerate, it will be used for later use.
[0022] 82.93 kg of water, 8.5 kg of pearl powder, and 0.1 kg of preservative KathonLXE were added in turn to the mixer container that had been weighed, and the stirring speed was 400 revolutions per minute. It should be noted that the pearl powder should be evenly sprinkled in, and the above adding and stirring time is 10...
Embodiment 2
[0023] Embodiment 2, take 5 kilograms of ethylene glycol by weighing, put into the container, and this container is fixed on the stirrer. Set the speed of the mixer at 300 revolutions per minute.
[0024] Sprinkle 0.5 kg of polyethylene oxide powder weighed in advance into the stirring ethylene glycol at a constant speed with a small spoon. The speed of adding is controlled at 0.05 kilograms per minute, promptly with the time of 10 minutes, above-mentioned polyoxyethylene powder is added in the container. Stop the mixer, check whether there is agglomerate in the material, if there is, continue to stir; if there is no agglomerate, it will be used for later use.
[0025] Will weigh 88.25 kg of water, 5 kg of pearl powder, 0.05 kg of preservative DMDMH, 0.6 kg of bright blue pigment, and 0.6 kg of red pigment, and add them to the starting mixer container in sequence, and the stirring speed is 300 revolutions per minute. The pearl powder should be evenly sprinkled in, and the ab...
Embodiment 3
[0026] Embodiment 3, take 10 kilograms of ethylene glycol by weighing, put into the container, and this container is fixed on the mixer. Set the speed of the mixer at 500 revolutions per minute.
[0027] Sprinkle 1 kg of polyethylene oxide powder weighed in advance into the stirring ethylene glycol at a constant speed with a small spoon. The speed of adding is controlled at 0.2 kilograms per minute, promptly with the time of 5 minutes, above-mentioned polyoxyethylene powder is added in the container. Stop the mixer, check whether there is agglomerate in the material, if there is, continue to stir; if there is no agglomerate, it will be used for later use.
[0028] 76.792 kg of weighed water, 12 kg of pearl powder, 0.1 kg of preservative DMDMH, 0.1 kg of bright blue pigment, and 0.008 kg of red pigment were added in turn to the starting mixer container, and the stirring speed was 500 revolutions per minute. The pearl powder should be evenly sprinkled in, and the above-mention...
PUM
Login to View More Abstract
Description
Claims