High-strength debris brick
A rubble and high-strength technology, applied in the direction of climate sustainability, sustainable waste treatment, solid waste management, etc., can solve the problems of land occupation, no literature reports, environmental pollution, etc., to save land, build factories quickly, and achieve high returns Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] 1. Stir the mixture consisting of 80% urban construction demolition waste and 20% cement first;
[0030] 2. Evenly mix and react additive No. 1 liquid and No. 2 liquid at a ratio of 1.5:1 to form a silica gel solution for later use;
[0031] 3. Add the silica gel slurry into the mixture according to the weight ratio of the silica gel slurry and the mixture at 14:100, and stir for 5 minutes to make it uniform;
[0032] 4. Sent to pressing equipment for pressing, forming and stacking;
[0033] 5. It can leave the factory after two times of water curing.
[0034] The strength is MU15, which can be used as load-bearing bricks.
Embodiment 2
[0036] 1. Stir the mixture consisting of 90% urban construction demolition waste and 10% cement first;
[0037] 2. Add 7.5 parts of No. 1 liquid to 100 parts of the mixture. The components of No. 1 liquid and the percentage of bulk density are 20% sodium silicate and 80% water, and mix well;
[0038] 3. Then add 5 parts of No. 2 liquid according to 100 parts of the mixture. The components of No. 2 liquid and the percentage of bulk density are 10% of sulfuric acid and 90% of water, and mix well;
[0039] 4. Sent to pressing equipment for pressing, forming and stacking;
[0040] 5. It can leave the factory after two times of water curing.
[0041] The strength is MU10, which can be used as non-load-bearing bricks.
Embodiment 3
[0043] 1. Stir the mixture consisting of 90% urban construction demolition waste and 10% lime evenly;
[0044] 2. Add 6 parts of No. 1 liquid to 100 parts of the mixture. The components and volumetric weight percentages of No. 1 liquid are 20% sodium silicate and 80% water;
[0045] 3. Then add 4 parts of No. 2 liquid according to 100 parts of the mixture. The components and volumetric percentages of No. 2 liquid are 10% of sulfuric acid and 90% of water;
[0046] 4. Sent to pressing equipment for pressing, forming and stacking;
[0047] 5. It can leave the factory after two times of water curing.
[0048] The strength is MU10, which can be used as non-load-bearing bricks.