Bamboo fibre and ramie fibre mixed spinning fabric and method for production thereof
A technology of ramie fiber and blended fabrics, which is applied in textiles, textiles, papermaking, fabrics, etc., and can solve problems such as dyed whiteness, wearing performance itching, and high cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] make 14 s ×14 s ×54×54×63 fabric.
[0016] Bamboo fiber and ramie fiber (short fiber) are selected at a ratio of 55:45, which are evenly stacked in the plucking machine, and rolled into rolls after being grasped, mixed, opened, and impurity removed, and the weight of the roll is controlled at 495±5 g / m; the roll is carded into strips, the speed of the carding licker-in roller is controlled at 750-900 rpm (900 rpm in this embodiment), the draft ratio is 107 times, and the carding sliver weighs 28.5 ± 0.5 g / min 5 meters; the sliver after carding is further evenly stretched on the drawing frame and combined into mature sliver, and the drawing draft ratio is controlled at 7.5-8.5 times (the present embodiment is 7.8 times), and the drawing process conditions are as follows: : 9×12(mm), front roller speed: 2000 rpm.
[0017] Spinning is that cooked sliver is spun into roving, and the spinning roving process condition is that the draft ratio of roving is controlled at 6.5-...
Embodiment 2
[0024] make 32 s ×32 s ×80×68×63 new ramie fabric.
[0025] Select bamboo fiber strips and ramie fiber strips (medium-length fibers), the ratio of which is 90:10, mix bamboo fiber strips and ramie strips on a carding machine, and evenly draft mature strips, and control the draft ratio of the combs at 7.5-9.5 times (the present embodiment is 8.5 times). The technological conditions are needle plate striking times: 852 times / minute, needle plate specification: 7-13 needles / hour, back tension: 1.013, front tension: 1.014.
[0026] Spinning is that cooked sliver is spun into roving, and the process condition of spinning head roving is that the draft ratio of roving is controlled at 6.5-8.5 times (the present embodiment is 8.5 times), spindle speed: 300 rpm, front roller speed: 185 rpm / min, the twist coefficient is 19; the process condition of spinning the second roving is that the draft ratio of the roving is controlled at 6.5-8.5 times (the present embodiment is 8.2 times), t...
Embodiment 3
[0032] make 7 s ×7 s ×72×44×60 twill denim fabric
[0033] Bamboo fiber and ramie fiber (short fiber) are selected at a ratio of 25:75, and they are evenly stacked in the plucking machine, and rolled into rolls after grasping, mixing, opening, and impurity removal, and the weight of the roll is controlled at 495±5 g / m; the roll is carded into strips, the speed of the carding licker-in roller is controlled at 750-900 rpm (900 rpm in this embodiment), the draft ratio is 107 times, and the carding sliver weighs 28.5 ± 0.5 g / min 5 meters; the sliver after carding is further evenly straightened on the drawing frame and combined into mature sliver, and the drawing draft ratio is controlled at 7.5-8.5 times (the present embodiment is 8 times), and the drawing process conditions are as follows: roller gauge : 9×12(mm), front roller speed: 2000 rpm.
[0034] Spinning is that cooked sliver is made into yarn through air spinning, and its process conditions are: opening roller speed 55...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com