Algaecides for fishing net and preparation method thereof
An algae inhibitor and fishing net technology, which is applied in the fields of botanical equipment and methods, herbicides, algaecides, biocides, etc. Promotion and application and other issues to achieve the effect of reducing breeding costs, saving manpower and time, and shortening the breeding cycle
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2008-05-21
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to a chemical composition, in particular to an anti-algae agent for fishing nets and a preparation method thereof. Background technique
[0002] my country's aquaculture industry is developing rapidly, in which a large number of fishing nets are used. Fishing nets are usually woven from wires made of polyethylene, polyvinyl chloride, polypropylene or nylon. According to the different breeding objects, the net wires are thick or thin, and the mesh holes are large or small, so as to be processed into various specifications of net cages, net boxes, net fences and fishing nets and other fishing nets and nets. Because the fishing net is soaked in water for a long time, it is extremely vulnerable to the erosion of algae, moss, fungus, barnacles, dragon fruit, mussels, oysters and amphipods, thereby shortening its service life. In order to solve this problem, it is necessary to organize manpower to clean and decontaminate the net frequ...
Examples
Embodiment 1
[0030] Get 10 grams of tetrachloroisophthalonitrile and add 15 grams of cosolvent propylene glycol and add 5 grams of water and 0.2 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 12 hours;
[0031] Take 5 grams of pyrithione, add 7 grams of cosolvent propylene glycol, add 2 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether, and mix them uniformly with a ball mill for 12 hours;
[0032] Get 5 grams of thiocyanomethane and add 7 grams of cosolvent propylene glycol and add 2 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether and mix evenly with a ball mill for 12 hours;
[0033] Add 50 grams of acrylic resin to 30 grams of water and mix well;
[0034] Take 0.3 grams of calcium polyacrylate and add 2 grams of water and mix well;
[0035] The above solutions are combined and stirred evenly, and the pH value is adjusted to 7.0-10.0 to obtain an anti-algae agent product for fishing nets o...
Embodiment 2
[0037] Get 5 grams of tetrachloroisophthalonitrile and add 10 grams of cosolvent propylene glycol and add 5 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 11 hours;
[0038] Take 10 grams of pyrithione, add 15 grams of cosolvent propylene glycol, add 8 grams of water and 0.2 grams of surfactant nonylphenol polyoxyethylene ether, and mix them uniformly with a ball mill for 11 hours;
[0039] Get 8 grams of thiocyanomethane and add 10 grams of cosolvent propylene glycol and add 5 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 11 hours;
[0040] Add 60 grams of acrylic resin to 40 grams of water and mix well;
[0041] Take 0.2 grams of calcium polyacrylate and add 2 grams of water to mix evenly;
[0042] The above solutions are combined and stirred evenly, and the pH value is adjusted to 7.0-10.0 to obtain an anti-algae agent product for fishing...
Embodiment 3
[0044] Get 15 grams of tetrachloroisophthalonitrile and add 20 grams of cosolvent propylene glycol and add 10 grams of water and 0.3 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 13 hours;
[0045] Take 2 grams of pyrithione, add 4 grams of cosolvent propylene glycol, add 2 grams of water and 0.05 grams of surfactant nonylphenol polyoxyethylene ether, and mix them uniformly with a ball mill for 13 hours;
[0046] Get 10 grams of thiocyanomethane and add 15 grams of cosolvent propylene glycol and add 10 grams of water and 0.2 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 13 hours;
[0047] Add 70 grams of acrylic resin to 50 grams of water and mix well;
[0048] Take 0.4 gram of polyacrylic acid calcium and add 2 grams of water and mix well;
[0049] The above solutions are combined and stirred evenly, and the pH value is adjusted to 7.0-10.0 to obtain an anti-algae agent product for fi...