[0027] A method for producing pearlescent yarn with 32s / l long-staple cotton + 80s / l long-staple cotton includes the following processing steps:
[0028] 1. Spinning
[0029] Spin high-quality long-staple cotton into 32s / l and 80s / l yarns respectively;
[0030] The twist of 32s / l coarse yarn is spun at the lowest equipment, the twist is 62 twists / 10CM, and the twist coefficient is 265;
[0031] The 80s / l fine yarn is spun with conventional knitting yarn twist, the twist is 130 twists / 10CM, and the twist coefficient is 350.
[0032] 2. Joint stock and line
[0033] According to the characteristics of the two-for-one twister, a thin yarn is wrapped and coiled around a thick yarn. The twist is 53 twists / 10CM, and the twist coefficient is controlled at 272.
Embodiment 2
[0035] A method for producing pearlescent colored cotton yarn with 40s / l dyed yarn + 80s / l compact spinning, including the following processing steps:
[0036] 1. Spinning
[0037] Spin high-quality long-staple cotton into 40s / l and 80s / l yarns respectively;
[0038] 40s / l thick yarn twist is spinning according to the lowest equipment, the twist is 53 twists / 10CM, and the twist coefficient is controlled at 272;
[0039] The 80s / l fine yarn is spun at the normal twist of the knitting yarn, the twist is 130 twists / 10CM, and the twist coefficient is 350.
[0040] 2. Single yarn dyeing
[0041] Dye 40s / l into colored yarn.
[0042] 3. Joint stock and line
[0043] According to the characteristics of the two-for-one twister, a thin yarn is wrapped and wound around a thick yarn. The twist is 58 twists / 10CM, and the twist coefficient is controlled at 272.
Embodiment 3
[0045] A method for producing pearlescent colored cotton yarn with 40s / l hemp cotton (90 / 10) + 80s / l spun cotton (75 / 25), including the following processing steps:
[0046] 1. Spinning
[0047] Choose high-quality linen cotton to spin 90 / 10 40s / l yarn, and high-quality spun cotton to spin 75 / 25 80s / l yarn;
[0048] The technical parameters of 40s / l yarn spinning for hemp / cotton 90 / 10, the twist is 53 twists / 10CM, and the twist coefficient is controlled at 272;
[0049] Spinning technical parameters for spun cotton 75 / 25 80s / l yarn, twist is 130 twists / 10CM, and twist coefficient is 350.
[0050] 2. Single yarn dyeing
[0051] Dye different colors with 40s / l for hemp cotton 90 / 10 and 80s / l for silk cotton 75 / 25.
[0052] 3. Joint stock and line
[0053] According to the characteristics of the two-for-one twister, a thin yarn is wrapped and wound around a thick yarn. The twist is 58 twists / 10CM, and the twist coefficient is controlled at 272.