Manufacturing method of steel rotational moulding pipeline with polyolefin lining layer
A manufacturing method and polyolefin technology, applied in the direction of coatings, pipes, rigid pipes, etc., can solve the problems of pipe section corrosion, easy corrosion, local corrosion of liquid or steam piping, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0037] Steel Rotomolded Polyolefin PO Pipes
[0038] Technical indicators:
[0039] A. DN65 steel rotationally molded polyolefin PO pipe, the pipe is 20#, the outer diameter is required to be ¢76mm, the steel pipe thickness is 3.5mm, the inner diameter is 76-7=69mm, the lining thickness is 3mm, and the length is 5 meters, including the flange surface .
[0040] B. Design pressure: PN1.0
[0041] C. The design temperature is 90°C.
[0042] D. Medium: 85% phosphoric acid solution.
[0043] E. Internal rotational molding polyolefin PO resin, thickness: 3mm±0.3mm.
[0044] Cutting: Cut a 5-meter-long steel pipe on the cutting machine.
[0045] Welding: Welding the flange to the pipe requires double-sided welding.
[0046] Grinding: Grind the solder joints of the welding place smoothly. If pores are found, repair welding is required in time.
[0047] Surface: remove welding slag, spatter and other attachments, and clean surface grease and soluble dirt.
[0048] Sand blasti...
Embodiment 2
[0058] Steel Rotomolded Polyolefin PO Pipes
[0059] Technical indicators:
[0060] A. DN400 steel rotationally molded polyolefin PO pipe, the pipe is 20#, the outer diameter is required to be ¢426mm, the steel pipe thickness is 9mm, and the standard GB / T8163 is implemented, the inner diameter is 426-18=408mm, the lining thickness is 7mm, and the length is 12 meters , including the flange surface.
[0061] B. Design pressure: PN1.0;
[0062] C. The design temperature is 90°C;
[0063] D. Medium: 50% sodium hydroxide solution;
[0064] E. Internal rotational molding polyolefin PO resin, thickness: 7mm±0.5mm;
[0065] Cutting: cut a 12-meter-long steel pipe on the cutting machine;
[0066] Welding: Welding flanges to pipes and fittings requires double-sided welding.
[0067] Grinding: Grind the solder joints of the welding place smoothly. If pores are found, repair welding is required in time.
[0068] Surface: remove welding slag, spatter and other attachments, and clea...
Embodiment 3
[0079] Steel Rotomolded Polyolefin PO Pipes
[0080] Technical indicators:
[0081] A. DN25 steel rotomolded polyolefin PO pipe, the pipe is 20#, the outer diameter is required to be ¢32mm, the steel pipe thickness is 2.5mm, the inner diameter is 32-5=27mm, the lining thickness is 2mm, and the length of each pipe is 2 meters. Lan noodles.
[0082] B. Design pressure: PN1.0;
[0083] C. The design temperature is 80°C;
[0084] D. Medium: concentrated sulfuric acid;
[0085] E. Internal rotational molding polyolefin PO resin, thickness: 2mm±0.2mm.
[0086] F. The shell material is 20# fluid seamless steel pipe, the thickness of the steel pipe is 2.5mm. The implementation standard is GB / T8163
[0087] Cutting: Cut a 2-meter-long pipe on the cutting machine.
[0088] Welding: Welding flanges to pipes and fittings requires double-sided welding.
[0089] Grinding: Grind the solder joints of the welding place smoothly. If pores are found, repair welding is required in time. ...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com