A flaky silver powder and anti-oxidation technology, which is applied in the field of flaky silver powder and its preparation, can solve the problems of affecting anti-counterfeiting performance, flaky silver powder is easy to oxidize, etc., and achieve the effect of improving anti-oxidation performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0051] Its content of the antioxidative flaky silver powder is specifically:
[0052] 6-8 micron flake silver powder 10 kg
[0053] 10 liters of high-purity water
[0054] Silver protectant 200g
[0055] Its preparation method is as follows:
[0056] a. Measure 10 liters of high-purity water, put the above-mentioned high-purity water in a container, and heat to 80°C;
[0057] b. Weigh 10 kg of flaky silver powder and 200 grams of silver protectant (EZ-AGII water-soluble silver protectant from Shenzhen Erzhen Technology Co., Ltd.) and place them in the above container;
[0058] c. Fully stir after soaking for 1 hour;
[0059] d. Pour the aqueous solution of the above-mentioned flaky silver powder into 5 drying trays, and set the oven temperature to 80°C;
[0060] e. Obtain anti-oxidation flaky silver powder after drying.
Embodiment 2
[0061] Embodiment 2: Its content of the flaky silver powder of described antioxidation is specifically:
[0062] 6-8 micron flake silver powder 10 kg
[0063] 10 liters of high-purity water
[0064] Silver Protectant 300g
[0065] Its preparation method is as follows:
[0066] a. Measure 10 liters of high-purity water, put the above-mentioned high-purity water in a container, and heat to 80°C;
[0067] b. Weigh 10 kg of flaky silver powder and 300 grams of silver protectant (EZ-AGII water-soluble silver protectant from Shenzhen Erzhen Technology Co., Ltd.) and place them in the above container;
[0068] c. Fully stir after soaking for 1 hour;
[0069] d. Pour the aqueous solution of the above-mentioned flaky silver powder into 5 drying trays, and set the oven temperature to 80°C;
[0070] e. Obtain anti-oxidation flaky silver powder after drying.
Embodiment 3
[0072] Its content of the antioxidative flaky silver powder is specifically:
[0073] 6-8 micron flake silver powder 10 kg
[0074] 10 liters of high-purity water
[0075] Silver Protectant 400g
[0076] Its preparation method is as follows:
[0077]a. Measure 10 liters of high-purity water, put the above-mentioned high-purity water in a container, and heat to 80°C;
[0078] b. Weigh 10 kg of flaky silver powder and 400 grams of silver protectant (EZ-AGII water-soluble silver protectant from Shenzhen Erzhen Technology Co., Ltd.) and place them in the above container;
[0079] c. Fully stir after soaking for 1 hour;
[0080] d. Pour the aqueous solution of the above-mentioned flaky silver powder into 5 drying trays, and set the oven temperature to 80°C;
[0081] e. Obtain anti-oxidation flaky silver powder after drying.