A production method, silver-gray technology, which is applied in the production of silver-gray matt projection/writing boards and the production of its baking paint, can solve the problems of affecting students' eyesight, unsightly appearance, short service life, etc., and achieve good visual effects , solve dust pollution, long service life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0056] (1) Ingredients
[0057] Accurately measure and take the following raw materials by weight in order: polyester resin D15530 parts; acrylic resin A1456 parts; acrylic resin XP26454 parts; 0.5 parts of Disponer904 dispersant, 0.5 part of Disponer983 dispersant, anti-settling agent 1 part and 7.3 parts of solvent were metered into the mixing barrel respectively.
[0058] (2) Mixing material
[0059] First mix all kinds of resins, solvents and various additives, then start the high-speed mixer, and at the same time turn on the cooling water, the temperature is controlled at less than 40°C, and then add carbon black FW-2000.1 parts according to the formula amount, phthalocyanine blue 0.1 part of BF401, 0.2 part of phthalocyanine green G5339D, 0.2 part of phthalocyanine green G5309H, after stirring for 10 minutes, add 150 parts of titanium dioxide TR8, 1 part of anti-settling agent, 7.3 parts of solvent, and continue stirring for 20 minutes until the surface of the pigment i...
Embodiment 2
[0066] (1) Ingredients
[0067] Accurately measure and take the following raw materials by weight in order: polyester resin D15520 parts; acrylic resin A1455 parts; acrylic resin XP26455 parts; 0.5 parts of Disponer904 dispersant, 0.5 parts of Disponer983 dispersant, anti-settling agent 1 part and 7.4 parts of solvent were metered into the mixing barrel respectively.
[0068] (2) Mixing material
[0069] First mix all kinds of resins, solvents and various additives, then start the high-speed mixer, and at the same time turn on the cooling water, the temperature is controlled at less than 40°C, and then add carbon black FW-2000. 0.2 parts of BF401, 0.1 part of phthalocyanine green G5339D, 0.1 part of phthalocyanine green G5309H and stir for 10 minutes, then add 160 parts of titanium dioxide TR8, and continue stirring for 20 minutes until the surface of the pigment is completely wetted and becomes a uniform paste without dry pigment. Stop stirring and turn off cooling water. ...
Embodiment 3
[0076] (1) Ingredients
[0077] Accurately measure and take the following raw materials in order by weight: polyester resin D15525 parts; acrylic resin A1458 parts; acrylic resin XP26455 parts; 0.2 parts of Disponer904 dispersant, 0.5 part of Disponer983 dispersant, anti-settling agent 1 part and 6 parts of solvent were metered into the mixing tank respectively.
[0078] (2) Mixing material
[0079] First mix all kinds of resins, solvents and various additives, then start the high-speed mixer, and at the same time turn on the cooling water, the temperature is controlled at less than 40°C, and then add carbon black FW-2000.1 parts according to the formula amount, phthalocyanine blue 0.3 parts of BF401, 0.1 part of phthalocyanine green G5339D, 0.1 part of phthalocyanine green G5309H, after stirring for 10 minutes, then add 140 parts of titanium dioxide TR8, 1-10 parts of anti-settling agent, and continue stirring for 20 minutes until the surface of the pigment is completely wet...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com