A kind of uv ink bridging agent and application thereof
A bridging agent and ink technology, applied in the field of ink printing, can solve the problems of easy falling off of UV ink patterns and excessive heavy metals in furniture, and achieve the effects of avoiding excessive heavy metals, good adhesion and enhanced adhesion.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] 1. Follow the steps below to print UV ink on the melamine board:
[0038] (1) Mix resin, curing agent and solvent according to the weight ratio of 1:0.5:0.8 to obtain bridging agent;
[0039] (2) Put the bridging agent into the spraying equipment for spraying, so that the bridging agent is sprayed onto the clean and dried melamine board;
[0040] (3) Dry the melamine board sprayed with bridging agent at room temperature for 60 minutes;
[0041] (4) Place the dried melamine board in a UV inkjet printer for ink spraying to obtain a sample board.
[0042] Wherein the resin comprises the following components by weight percentage: 45% cottonseed oil modified alkyd resin, 20% nitrocellulose, 28% ethyl acetate, 0.5% tetrafluoroethylene gas phase wax, 6.5% ethylene glycol ethyl ether monobutyl ester ; Curing agent contains 50% low free TDI curing agent raw material, 50% ethyl acetate; butyl ester.
[0043] 2. Formaldehyde content test
[0044] According to GB / T18584-2004, ...
Embodiment 2
[0056] 1. Follow the steps below to print UV ink on the melamine board:
[0057] (1) Mix the resin, curing agent and solvent according to the weight ratio of 1.5:0.25:0.5 to obtain the bridging agent;
[0058] (2) Put the bridging agent into the spraying equipment for spraying, so that the bridging agent is sprayed onto the clean and dried melamine board;
[0059] (3) Dry the melamine board sprayed with bridging agent at room temperature for 60 minutes;
[0060] (4) Place the dried melamine board in a UV inkjet printer for ink spraying to obtain samples.
[0061]Wherein the resin comprises the following components by weight percentage: 40% soybean oil modified alkyd resin, 29.4% nitrocellulose, 25% ethyl acetate, 1% paraldehyde, 0.6% tetrafluoroethylene gas phase wax, 4% Ethylene glycol ethyl ether monobutyl ester; curing agent contains 70% low free TDI curing agent raw material, 30% ethyl acetate; solvent includes the following components in weight percentage: 85% ethyl ace...
Embodiment 3
[0075] 1. Follow the steps below to print UV ink on the melamine board:
[0076] (1) Mix the resin, curing agent and solvent in a weight ratio of 1.5:0.75:0.5 to obtain a bridging agent;
[0077] (2) Put the bridging agent into the spraying equipment for spraying, so that the bridging agent is sprayed onto the clean and dried melamine board;
[0078] (3) Dry the melamine board sprayed with bridging agent at room temperature for 60 minutes;
[0079] (4) Place the dried melamine board in a UV inkjet printer for ink spraying to obtain samples.
[0080] Wherein the resin comprises the following components by weight percentage: 30% soybean oil modified alkyd resin, 30% nitrocellulose, 30% ethyl acetate, 1% tetrafluoroethylene gas phase wax, 8% ethylene glycol ethyl ether monobutyl ester and 1% polyether modified polydimethylsiloxane; the curing agent contains 60% low free TDI curing agent raw material, 40% ethyl acetate; the solvent includes the following components in weight per...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com