Embodiment 1
[0015] Step 1: Add 25g of raw materials containing catalyst alumina and 100mL of ethanol solution into a reaction kettle equipped with a stirrer, reflux condenser and thermometer, start stirring, adjust the heating voltage between 150 and 200V, and react for 0.5 after the temperature is constant. hours, the solid phase material is extracted after the reaction, and the liquid phase material is collected to be recycled;
[0016] Step 2: Put the solid phase material into the reaction kettle, add 100g of sodium hydroxide, ethanol and water mixture, wherein the mass fraction of sodium hydroxide is 5%, start stirring, keep the temperature in the reaction kettle at 85°C, heat After reacting for 0.5 hours, the solid phase material was extracted again, the solid phase material was washed twice, and the liquid phase material was collected for recycling;
[0017] Step 3: The solid-phase material obtained in Step 2 is repeatedly treated once according to the method of Step 2 to obtain a c...
Embodiment 2
[0019] The difference from Example 1 is that the catalyst alumina raw material added in step 1 is 28g, and the product purity is measured by roasting method, and the purity reaches 96.2%.
Embodiment 3
[0021] The difference from Example 1 is that the catalyst alumina raw material added in step 1 is 33g, and the product purity is measured by roasting method, and the purity reaches 96.1%.