A method for improving the hue of granular iron oxide black pigment
A technology of iron oxide black and pigments, applied in the field of chemical pigments, which can solve the problems of increased usage, high transportation costs, and poor tinting power, and achieve the effects of reduced production costs, simple manufacturing process, and improved tinting power
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] Embodiment 1 (taking 1000kg iron oxide black as experimental quantity):
[0026] 1) Take by weighing 0.4% sodium silicate of iron oxide black mass, i.e. 4kg sodium silicate, dissolve sodium silicate in water with a temperature of 40-50 degrees Celsius, and dissolve for 3 hours to prepare 80kg of sodium silicate aqueous solution;
[0027] 2) 0.08% sodium polynaphthalene sulfonate of iron oxide black quality, i.e. 0.008% urea of 0.008% polynaphthaldehyde sodium sulfonate and iron oxide black quality, i.e. 0.08kg urea is added in the sodium silicate solution, fully Stir for 10 minutes;
[0028] 3) Turn on the disc granulator, control the speed of the ball forming machine at 20-25 rpm, start adding iron oxide black powder at a speed of 35-50kg / min, and turn on the atomizing nozzle to adjust the spray angle of the atomizing nozzle to 130 ° to increase the spraying range;
[0029] 4) The granulation time is controlled at about 30 minutes, and the moisture content of the ...
Embodiment 2
[0036] Embodiment 2 (taking 1000kg iron oxide black as experimental quantity):
[0037] 1) Take by weighing 0.8% sodium silicate of iron oxide black mass, i.e. 8kg sodium silicate, dissolve sodium silicate in water with a temperature of 40-50 degrees Celsius, and dissolve for 3 hours to prepare 80kg of sodium silicate aqueous solution;
[0038] 2) 0.16% sodium polynaphthalene sulfonate of iron oxide black quality, i.e. 0.016% urea of 1.6kg polynaphthaldehyde sodium sulfonate and iron oxide black quality, i.e. 0.16kg urea is added in the sodium silicate solution, fully Stir for 10 minutes;
[0039] 3) Turn on the disc granulator, control the speed of the ball forming machine at 20-25 rpm, start adding iron oxide black powder at a speed of 35-50kg / min, and turn on the atomizing nozzle to adjust the spray angle of the atomizing nozzle to 130 ° to increase the spraying range;
[0040] 4) The granulation time is controlled at about 30 minutes, and the moisture of the final iro...