A kind of preparation method of high-strength conductive polymer nanocomposite material

A technology of nanocomposite materials and conductive polymers, applied in the direction of conductive materials dispersed in non-conductive inorganic materials, nanotechnology, etc., can solve problems such as poor dispersion, easy aggregation of metal nanowires, easy formation of secondary particles, etc., to achieve Good dispersibility and rheology, improve surface structure, reduce the effect of mutual attraction

Inactive Publication Date: 2018-01-12
SOUTHWEAT UNIV OF SCI & TECH
View PDF3 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0006] The present invention aims to overcome the deficiencies of the prior art, solve the problems of easy aggregation, poor dispersion, and easy formation of secondary particles of metal nanowires by using dopamine coating modification, and provide a high-strength conductive polymer nanocomposite preparation method

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A kind of preparation method of high-strength conductive polymer nanocomposite material
  • A kind of preparation method of high-strength conductive polymer nanocomposite material

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0032] Step 1. Add the metal nano-silver wire into water and fully shake and dissolve at a speed of 200r / min to prepare a 0.01mol / L metal nano-silver wire solution. Take 50mL of the metal nano-silver wire solution and add trihydric acid with a concentration of 2mg / mL Methylaminomethane solution 1mL, adjust the pH to 8.5 with dilute hydrochloric acid, add 1mL dopamine solution with a concentration of 1mg / mL, and fully stir and react at a speed of 300r / min for 5h to obtain a dopamine-coated metal nanosilver wire solution; figure 1 A scanning electron microscope image of a dopamine-coated metal nanosilver wire is shown;

[0033] Step 2: Inject the obtained dopamine-coated metal nano-silver wire solution into a polytetrafluoroethylene tubular mold with a height of 3 cm and a diameter of 3 cm. The bottom of the polytetrafluoroethylene tubular mold is fixed on the steel plate, and the steel plate is placed on Freeze in liquid nitrogen at -196°C. After the dopamine-coated metal nanos...

Embodiment 2

[0037] Step 1. Add metal nano-silver wire into water and fully shake and dissolve at a speed of 200r / min to prepare a 0.03mol / L metal nano-silver wire solution. Take 50mL of metal nano-silver wire solution and add trihydric acid with a concentration of 4mg / mL Methyl aminomethane solution 1mL, adjust the pH to 8.5 with dilute hydrochloric acid, add 1mL dopamine solution with a concentration of 2mg / mL, and fully stir and react at a speed of 300r / min for 6h to obtain a dopamine-coated metal nanosilver wire solution;

[0038] Step 2: Inject the obtained dopamine-coated metal nano-silver wire solution into a polytetrafluoroethylene tubular mold with a height of 3 cm and a diameter of 3 cm. The bottom of the polytetrafluoroethylene tubular mold is fixed on the steel plate, and the steel plate is placed on Freeze in liquid nitrogen at -196°C. After the dopamine-coated metal nanosilver wire solution is completely frozen, place it in a freeze dryer and dry it for 72 hours at a temperatu...

Embodiment 3

[0042] Step 1. Add metal nano-silver wires into water and fully oscillate and disperse at a speed of 200r / min to prepare a 0.05mol / L metal nano-silver wire solution. Take 50mL of metal nano-silver wire solution and add trihydric acid with a concentration of 5mg / mL Methylaminomethane solution 1mL, adjust the pH to 8.5 with dilute hydrochloric acid, add 1mL dopamine solution with a concentration of 4mg / mL, and fully stir and react at a speed of 300r / min for 8h to obtain a dopamine-coated metal nanosilver wire solution;

[0043] Step 2: Inject the obtained dopamine-coated metal nano-silver wire solution into a polytetrafluoroethylene tubular mold with a height of 3 cm and a diameter of 3 cm. The bottom of the polytetrafluoroethylene tubular mold is fixed on the steel plate, and the steel plate is placed on Freeze in liquid nitrogen at -196°C. After the dopamine-coated metal nanosilver wire solution is completely frozen, place it in a freeze dryer and dry it for 96 hours at a tempe...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
diameteraaaaaaaaaa
tensile strengthaaaaaaaaaa
tensile strengthaaaaaaaaaa
Login to View More

Abstract

The invention discloses a preparation method of a high-strength conductive polymer nanocomposite. The preparation method comprises the following steps: (1) preparing a metal nanowire solution, adding a tris(hydroxymethyl)aminomethane solution, adjusting the pH value with diluted hydrochloric acid, adding a dopamine solution, and stirring for reacting to obtain a dopamine-coated metal nanowire solution; (2) injecting the dopamine-coated metal nanowire solution into a polytetrafluoroethylene tubular mould, fixing the bottom of the polytetrafluoroethylene tubular mould on a steel plate, and freezing the steel plate in liquid nitrogen; after the dopamine-coated metal nanowire solution is completely frozen, drying in a freeze dryer to form a metal nanowire network structure; and (3) heating the polymer material into a completely molten state, and injecting into the metal nanowire network structure to obtain a high-strength macro-scale polymer conductive material. In the invention, the metal nanowire can improve the polymer conductivity; and as inorganic filler, the metal nanowire can effectively enhance the polymer mechanical properties.

Description

technical field [0001] The invention belongs to the field of preparation of high-molecular conductive materials, and in particular relates to a preparation method of high-strength conductive high-molecular nanocomposite materials. Background technique [0002] Conductive polymer nanocomposites integrate the properties of polymers and the functionality of nanoparticles, and have a strong application background, thus rapidly becoming an important research direction in the field of nanocomposites. Composite conductive materials are made by adding conductive materials such as metal powder or metal wires to resin after physical modification. Polymer materials such as epoxy resin and polyimide are not conductive by themselves, but they have good conductive properties after being doped with metal nanowires. [0003] Nanowires have been paid more and more attention due to their excellent properties. Because metal nanomaterials combine the properties of nanomaterials and metal mate...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): C08L63/00C08L79/08C08K9/10C08K7/06B22F9/24B82Y40/00H01B1/22
CPCB22F9/24B82Y40/00C08K7/06C08K9/10C08K2201/001C08K2201/011C08L2201/08H01B1/22C08L63/00C08L79/08
Inventor竹文坤段涛姚卫棠周磊雷佳
OwnerSOUTHWEAT UNIV OF SCI & TECH