A ceramic with invisible anti-counterfeiting function
A ceramic and functional technology, applied in the field of ceramics, can solve the problems of poor anti-counterfeiting effect, easy damage and counterfeiting
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] 1) Mix high-temperature china clay and anti-counterfeiting powder (Youpinbao Technology (Technology) Beijing Co., Ltd.) in a ratio of 100:0.3 to prepare anti-counterfeiting china clay;
[0028] 2) Stir the anti-counterfeiting porcelain clay mixture prepared in step 1), add water with a mass fraction of 8%, water glass with a mass fraction of 3‰, and American fairy water with a mass fraction of 1‰, then stir it with a fast beater for 1 hour, and then use a 120-mesh Sieve filtration to obtain a flow rate of 25m / s and a specific gravity of 160g / cm 3 mud;
[0029] 3) Pour the mud obtained in step 2) into a gypsum mold, wait for 30 minutes to solidify the mud, and take out the mud;
[0030] 4) After step 3) is completed, the mud is naturally dried for more than 24 hours, and then repaired;
[0031] 5) Put the mud base that has been repaired in step 4) into a kiln for biscuit firing, and burn it to 700 ° C for 5 hours;
[0032] 6) Glazing the biscuit obtained in step 5), a...
example 2
[0035] 1) Mix high-temperature china clay and anti-counterfeit powder according to the ratio of 100::1 to prepare anti-counterfeit china clay;
[0036] 2) Stir the anti-counterfeiting porcelain clay mixture prepared in step 1), add water with a mass fraction of 10%, water glass with a mass fraction of 3.5‰, and American fairy water with a mass fraction of 2‰, then stir with a fast beater for 2 hours, and then use a 150-mesh Sieve filtration to obtain a flow rate of 28m / s and a specific gravity of 170g / cm 3 mud;
[0037] 3) Pour the mud obtained in step 2) into a gypsum mold, wait for 40 minutes to solidify the mud, and take out the mud;
[0038] 4) After step 3) is completed, the mud is naturally dried for more than 24 hours, and then repaired;
[0039] 5) Put the mud base that has been repaired in step 4) into a kiln for biscuit firing, and burn it to 750 ° C for 5 hours;
[0040] 6) Glaze the biscuit obtained in step 5), and perform high-temperature reduction firing on th...
example 3
[0043] 1) Mix high-temperature china clay and anti-counterfeit powder according to the ratio of 100:1.5 to prepare anti-counterfeit china clay;
[0044] 2) Stir the anti-counterfeit porcelain clay mixture prepared in step 1), add water with a mass fraction of 12%, water glass with a mass fraction of 4‰, and American fairy water with a mass fraction of 3‰, then stir with a fast beater for 3 hours, and then use a 180-mesh Sieve filtration to obtain a flow rate of 30m / s and a specific gravity of 180g / cm 3 mud;
[0045] 3) Pour the mud obtained in step 2) into a gypsum mold, wait for 50 minutes to solidify the mud, and take out the mud;
[0046] 4) After step 3) is completed, the mud is naturally dried for more than 24 hours, and then repaired;
[0047] 5) Put the mud base that has been repaired in step 4) into a kiln for biscuit firing, and burn it to 800 ° C for 5 hours;
[0048] 6) Glaze the biscuit obtained in step 5), and reduce the glazed body to high-temperature reductio...
PUM
Property | Measurement | Unit |
---|---|---|
spectroscopy | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com