[0009] Based on this, the present invention provides a papermaking method, which can increase the adsorption rate of starch on the fiber surface or in pulp, thereby increasing the retention rate of starch i...

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Papermaking method
  • Papermaking method
  • Papermaking method

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0340] Example 1 Effect of cationic starch binder cetylpyridine hydrochloride (number C7) on starch dissolution and fiber surface adsorption after reacting with starch

[0341] Experimental steps: (1) take cornstarch sample and prepare 7% "standard starch solution"; (2) take an appropriate amount of standard starch solution and add deionized water to dilute to the required concentration of starch solution; (3) take the prepared concentration Put 500mL of starch solution in a beaker, and put it into a 45°C constant temperature water bath, and equilibrate to the specified temperature; (4) Add C7 according to the required concentration, and react for 60 minutes to obtain a modified starch solution; (5) Sampling and centrifuging ( 4000x g) for 5 minutes, take the supernatant to test the starch concentration; (6) add bleached chemical pulp (BKP) to the remaining modified starch solution according to a solid concentration of 1%, and keep stirring for 10 minutes; (7) after the reactio...

Embodiment 2

[0348] The impact of embodiment 2 reaction time on starch binding reaction

[0349] Experimental steps of starch reaction: (1) take corn starch sample and prepare 7% "standard starch solution"; (2) take appropriate amount of standard starch solution and dilute it with deionized water to a starch concentration of about 1800mg / L (or other required concentration) (3) Take 500mL of the prepared starch solution or OCC white water, place it in a beaker, and put it into a 45°C constant temperature water bath, and equilibrate to the specified temperature; (4) Add 30mg / L starch binder as required, When the reaction reaches 1, 3, 5, 10, 30, 60, 90, 120, 300, 600 and 1200 minutes, the sample is centrifuged (4000x g) for 5 minutes, and the supernatant is taken to test the starch content and COD concentration;

[0350] The test procedure of starch adsorption reaction time: steps (1)-(4) are the same as above, (5) when the starch reaction reaches 60 minutes, add 3% chemical pulp (BKP) accor...

Embodiment 3

[0355] Embodiment 3 Reaction temperature is to the influence of starch binding reaction and the adsorption effect of modified starch

[0356] Experimental steps: (1) Take corn starch samples to prepare 7% "standard starch solution"; (2) Take an appropriate amount of standard starch solution and add deionized water to dilute to a starch concentration of about 600mg / L; (3) Take the prepared starch solution 500mL, placed in a beaker, and put into a constant temperature water bath with the required test temperature preset, and equilibrated to the specified temperature; (4) According to the requirements of the test, add 30mg / L cationic starch binder C7 and react for 60 minutes to obtain Modified starch solution; (5) sample centrifugation (4000x g) for 5 minutes, get the supernatant to test starch content and COD concentration; (6) add chemical pulp (BKP ) (Note: The amount of starch binder is equivalent to 1000g / T dry pulp), keep stirring; (7) React for 10 minutes, take the slurry ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
Viscosityaaaaaaaaaa
Burst indexaaaaaaaaaa
Login to view more

Abstract

The present invention relates to a papermaking method. The papermaking method comprises the following steps: (a) a cation starch complex agent is added into starch-containing pulping white water or astarch aqueous solution to react, and a modified starch solution is obtained; (b) fibers or paper pulp is added into the modified starch solution and stirred, an adsorption reaction is conducted, andpulp subjected to reaction is obtained; and (c) the pulp subjected to reaction is prepared to form a paper product, wherein the chemical structure of the cation starch complex agent is composed of thefollowing parts: (i) one or more hydrophobic groups and (ii) one or more hydrophilic groups, the one or more hydrophobic groups can react with starch to produce an inclusion complex, and the hydrophilic groups and the hydrophilic groups are located at the two ends of the same molecular structure correspondingly and connected through chemical bonds to form the asymmetrical and polar structure. According to the papermaking method, the adsorption rate of the starch on the surfaces of the fibers or in the paper pulp can be increased, thus the retention rate of the starch in paper is increased, and COD emission is lowered.

Description

technical field [0001] The invention relates to the technical field of papermaking, in particular to a papermaking method. Background technique [0002] The entire production process of the pulp and paper industry, including from material preparation to paper making, chemical recycling, and paper processing, requires a large amount of water for conveying, washing, dispersing materials, and cooling equipment. Although there are recycling, treatment, and reuse in the production process, a large amount of waste water is still discharged into the water body, causing serious pollution to the water environment. Worldwide, paper industry wastewater is an important source of pollution. For example, Japan and the United States list paper industry wastewater as one of the six major public hazards and one of the five major public hazards. [0003] At present, my country's paper industry wastewater discharge and COD discharge rank first in all types of industrial emissions in my countr...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): D21F11/00D21H17/29
CPCD21F11/00D21H17/29
Inventor 王祥槐张福山李志军胡维维
Owner RISINGSTAR BIOTECH GUANGZHOU
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products